Surface treatment liquid, mica tube and preparation method thereof
By using a surface treatment liquid with a specific ratio and a two-stage drying process, the problems of gaps, roughness, and high-temperature cracking in mica tubes have been solved, achieving high fire resistance and insulation properties for mica tubes, making them suitable for insulation layers in electrical equipment.
Patent Information
- Application Number
- CN202311106955.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-08-30
AI Technical Summary
Traditional mica tube manufacturing methods result in gaps at the joints, affecting insulation performance. Furthermore, the extrusion molding method leads to a rough surface that is prone to powdering, cracking at high temperatures, and insufficient fire resistance and insulation.
A surface treatment liquid composed of ceramic powder, silica, glass powder and organosilicon resin in a specific ratio is used to form a ceramic-like coating. Combined with extrusion molding and a two-stage drying process, mica tubes are prepared.
The fire resistance and electrical insulation of mica tubes have been improved, enabling them to withstand voltages ≥55kV and fire resistance temperatures >900℃ at room temperature, meeting the requirements for use as insulation layers for electrode rods or waterproof sleeves.
Smart Images

Figure BDA0004422466340000051 
Figure BDA0004422466340000052 
Figure BDA0004422466340000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrical insulation materials, and in particular to a surface treatment liquid, a mica tube and a preparation method thereof. Background Art
[0002] Mica tube is a hard plastic tubular material made of mica. It has excellent thermal insulation properties and mechanical strength. Therefore, it is often used to make electrode rods or out-of-bounds waterproof casing insulation layers in various household appliances, motors, electric smelting furnaces and other machinery and equipment.
[0003] The traditional method of preparing mica tubes is to immerse mica paper in an organic chemical binder, and after the binder is dried, the mica paper is rolled, dried and shaped to obtain a mica tube. However, there are gaps at the joints of the mica tubes obtained by this method, which may seriously affect the insulation performance of the mica tubes. In recent years, researchers have developed a method for preparing mica tubes by extrusion molding. Although the mica tubes obtained by this method are seamless, the surface of the mica tubes is rough and easy to fall off. In addition, the mica tubes have the problem of cracking at high temperatures, which seriously affects the fire resistance and insulation of the mica tubes. Summary of the invention
[0004] In order to improve the fire resistance and electrical insulation of mica tubes, the present application provides a surface treatment liquid, a mica tube and a preparation method thereof.
[0005] In the first aspect, the present application provides a surface treatment liquid, which adopts the following technical solution:
[0006] A surface treatment liquid comprises the following components in parts by weight: 15-25 parts of ceramic powder, 35-55 parts of silicon dioxide, 5-15 parts of glass powder and 35-45 parts of organic silicon resin.
[0007] In the present application, a surface treatment liquid is applied to the outer surface of the mica tube, and after the surface treatment liquid is cured, a vitrified coating can be formed on the outer surface of the mica tube, and the vitrified coating will be vitrified and transformed into a hard and stable ceramic layer at a high temperature above 600°C, thereby further improving the fire resistance and insulation of the mica tube. In the present application, it is found through experimental research that the addition amount of each component of the surface treatment liquid will affect the fire resistance and insulation and surface performance of the mica tube at high temperature. Specifically, when the added amount of ceramic powder is less than 15 parts, the insulation of the mica tube is poor; when the added amount of ceramic powder is greater than 25 parts, the surface of the mica tube is rough and there is a small amount of powder falling off; when the added amount of silica is less than 35 parts, the uniformity of the surface treatment liquid is poor, and the ceramic coating formed by curing is uneven; when the added amount of silica is greater than 55 parts, the surface of the mica tube is rough and there is a small amount of powder falling off; when the added amount of glass powder is less than 5 parts, the ceramic coating is easy to fall off at high temperature; when the added amount of glass powder is greater than 15 parts, the outer surface of the mica tube is uneven; when the added amount of silicone resin is less than 35 parts, the silicone resin cannot fill the surface of the mica tube, so the surface of the mica tube is rough; when the added amount of silicone resin is greater than 45 parts, the surface of the mica tube cannot be cured into a ceramic coating. Therefore, the present application controls the addition amount of each component in the surface coating treatment liquid within the above-mentioned range, and can obtain a surface coating treatment liquid with good uniformity, high temperature resistance and excellent electrical insulation. The above-mentioned surface coating treatment liquid is used to coat the outer surface of the mica tube, which can form a flat and firm vitrified coating on the outer surface of the mica tube, thereby further improving the fire resistance and electrical insulation of the mica tube.
[0008] In a specific embodiment, the weight portion of the ceramic powder may be 10 parts, 20 parts or 25 parts.
[0009] In a specific embodiment, the weight parts of the silicon dioxide may be 35 parts, 40 parts or 55 parts.
[0010] In a specific embodiment, the weight proportion of the glass powder may be 5 parts, 10 parts or 15 parts.
[0011] In a specific embodiment, the weight parts of the silicone resin may be 35 parts, 40 parts or 45 parts.
[0012] Preferably, the surface treatment liquid comprises the following components in parts by weight: 20 parts of ceramic powder, 40 parts of silicon dioxide, 10 parts of glass powder and 40 parts of silicone resin.
[0013] A preparation method of a surface treatment liquid comprises the following steps: mixing various components, and stirring at a stirring speed of 500-800 r / min for 60-100 min to obtain the surface treatment liquid.
[0014] Optionally, the silicone resin is selected from one or more of amino silicone resin, epoxy-modified silicone resin, acrylic-modified silicone resin and polyester-modified silicone resin.
[0015] Preferably, the silicone resin is a mixture of an amino silicone resin and an epoxy-modified silicone resin.
[0016] Further preferably, the weight ratio of the amino silicone resin to the epoxy modified silicone resin is 1:(0.35-0.75).
[0017] Through experimental research, the present application found that by preparing a surface treatment liquid with a mixture of amino silicone resin and epoxy modified silicone resin in a weight ratio of 1: (0.35-0.75), the surface flatness of the mica tube obtained is better and the fire-resistant temperature can reach above 1000°C.
[0018] In a specific embodiment, the weight ratio of the amino silicone resin to the epoxy-modified silicone resin may be 1:0.25, 1:0.35, 1:0.5, 1:0.75 or 1:0.9.
[0019] In a second aspect, the present application provides a mica tube.
[0020] A mica tube, the outer surface of which comprises a ceramic coating formed by the surface treatment liquid.
[0021] In the present application, by coating the surface of the extruded mica tube with a surface treatment liquid, the surface treatment liquid can form a fireproof, insulating, vitrified coating on the outer surface of the mica tube, thereby making the mica tube have better fire resistance and insulation.
[0022] Preferably, the thickness of the porcelainizable coating is 0.2±0.03 mm.
[0023] In a third aspect, the present application provides a method for preparing a mica tube, comprising the following steps: preparing a mica tube preform, coating, and drying; the drying adopts a two-stage drying process; the first stage drying temperature is 80-100°C, and the drying time is ≥8min; the second stage drying temperature is 150-170°C, and the drying time is ≥10min.
[0024] In the present application, the drying temperature will affect the surface performance and physical properties of the mica tube. Specifically, when the first stage drying temperature is higher than 100°C, bubbles appear on the surface of the mica tube. When the second stage drying temperature is lower than 150°C, the surface treatment liquid cannot be solidified and formed; when the second stage drying temperature is higher than 170°C, bubbles appear on the surface of the mica tube. Therefore, the present application controls the temperature and time in the drying process within the above range, and the surface treatment liquid can be solidified to form a stable ceramic coating, and the surface of the ceramic coating is smooth and free of bubbles, and the mica tube has excellent fire resistance and insulation properties.
[0025] In a specific embodiment, the drying temperature in the first stage can be 80°C, 90°C or 100°C.
[0026] In a specific embodiment, the second stage drying temperature may be 150°C, 160°C or 170°C.
[0027] In a specific embodiment, the first stage drying temperature is 90°C, and the second stage drying temperature is 160°C.
[0028] In the present application, the specific steps of preparing the mica tube preform are: extruding the mica material composition at an extrusion temperature of 170-190° C., and then air-cooling at 20-30° C. for ≥20 min to obtain the mica tube preform.
[0029] Preferably, in the coating step: the coating amount of the surface treatment liquid is 33-38 g / m 2 .
[0030] The present application controls the coating amount of the surface treatment liquid within the above range, and the thickness of the obtained porcelain coating is 0.2±0.03mm. The thickness of the porcelain coating of the above thickness is appropriate, will not fall off, and can significantly improve the fireproof and insulation properties of the mica tube.
[0031] In summary, this application has the following beneficial effects:
[0032] 1. The present application adopts a specific ratio of ceramic powder, silicon dioxide, glass powder and silicone resin to prepare a surface treatment liquid with excellent fire resistance and electrical insulation properties; the surface treatment liquid is applied to the outer surface of the mica tube, and the surface treatment liquid will become a fireproof, insulating, dense and vitrified coating after curing, thereby significantly improving the fire resistance and electrical insulation of the mica tube, making it withstand a voltage of ≥55kv at room temperature and a fire resistance temperature of >900℃, which can meet the use requirements of electric batons or waterproof casing insulation layers.
[0033] 2. The present application further uses amino silicone resin and epoxy modified silicone resin in a weight ratio of 1: (0.35-0.75) to prepare the surface treatment liquid, and the fire-resistant temperature of the obtained mica tube can reach above 1000°C.
[0034] 3. The present application provides a method for preparing a mica tube, which adopts a preparation process of extrusion molding + surface coating + two-stage drying. In the two-stage drying process, the first-stage drying temperature is controlled within the range of 80-100°C, and the second-stage drying temperature is controlled within the range of 150-170°C. The obtained mica tube is seamless and has a smooth surface, and the mica tube has no powder loss, high-temperature cracking, etc. The mica tube has excellent fire resistance and insulation properties. DETAILED DESCRIPTION
[0035] In a first aspect, the present application provides a surface treatment liquid, which comprises the following components in parts by weight: 15-25 parts of ceramic powder, 35-55 parts of silicon dioxide, 5-15 parts of glass powder and 35-45 parts of silicone resin. The silicone resin is selected from one or more of amino silicone resin, epoxy modified silicone resin, acrylic modified silicone resin and polyester modified silicone resin. Preferably, the silicone resin is a mixture of amino silicone resin and epoxy modified silicone resin; the weight ratio of the amino silicone resin to the epoxy modified silicone resin is 1:(0.35-0.75).
[0036] The preparation method of the surface treatment liquid is as follows: the components are mixed and stirred at a stirring speed of 500-800 r / min for 60-100 min to obtain the surface treatment liquid.
[0037] In a second aspect, the present application provides a mica tube, and a method for preparing the mica tube comprises the following steps:
[0038] (1) Preparation of mica tube preform:
[0039] (1-1) Preparing mica slurry: Mix the mica material composition evenly and stir it at a stirring speed of 600-1000 r / min for 80-120 min to obtain mica slurry; wherein the mica material composition comprises the following components in parts by weight: 75 parts of mica powder, 50 parts of polyethylene, 55 parts of silicon micropowder and 25 parts of organic silica gel.
[0040] (1-2) Extrusion molding: extruding the mica slurry at an extrusion temperature of 170-190° C., and then air-cooling at 20-30° C. for 20-60 min to obtain a mica tube preform;
[0041] (2) Coating: Then, the surface treatment liquid is coated on the surface of the mica tube preform. The coating amount of the surface treatment liquid is 33-38 g / m 2 .
[0042] (3) Drying: A double-stage drying process is used to dry the mica tube. In the double-stage drying process, the first stage drying temperature is 80-100°C and the drying time is ≥8 minutes; the second stage drying temperature is 150-170°C and the drying time is ≥10 minutes.
[0043] The sources of the raw materials used in the examples of this application are as follows:
[0044] Mica powder (purchased from Lingshou County Baofeng Mica Processing Co., Ltd.);
[0045] The model of polyethylene is HDPE 5000S (purchased from Yanshan Petrochemical);
[0046] Silica powder (purchased from Anhui Green New Materials Technology Co., Ltd.);
[0047] Organic silica gel (purchased from Hubei Xinsihai Chemical Co., Ltd.);
[0048] The ceramic powder is aluminum nitride powder, model AIN-H, (purchased from Liaoning Desheng Special Ceramics Manufacturing Co., Ltd.);
[0049] Silicon dioxide was fumed silicon dioxide (purchased from Shouguang Changtai New Materials Co., Ltd.);
[0050] Glass powder (1500 mesh, purchased from Hebei Wensheng New Material Technology Co., Ltd.);
[0051] Silicone resin: CS-2000 amino silicone resin (purchased from Wuxi Xiano New Material Technology Co., Ltd.), epoxy modified silicone resin (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.), acrylic modified silicone resin (purchased from Hubei Longsheng Sihai New Materials Co., Ltd.), polyester modified silicone resin (purchased from Wuhan Kemik Biomedical Technology Co., Ltd.).
[0052] In the present application, other raw materials, reagents, solvents, etc. can also be obtained through commercial purchase.
[0053] The present application is further described in detail below in combination with preparation examples, embodiments, and performance testing experiments.
[0054] Preparation Example 1-9
[0055] Preparation Examples 1-9 provide a surface treatment solution respectively. The difference between the above surface treatment solutions is that the amount of each component of the surface treatment solution is as shown in Table 1 below.
[0056] The preparation method of the surface treatment liquid provided in Preparation Example 1-9 is: weigh and mix the components according to the addition amount in Table 1, stir the components of the surface treatment liquid at a rate of 600 r / min for 60 minutes to obtain the surface treatment liquid.
[0057] Table 3 Components and addition amounts of the surface treatment liquid provided in Preparation Examples 1-9
[0058]
[0059] Comparative Preparation Examples 1-8
[0060] Comparative Preparation Examples 1-8 were prepared according to the method of Preparation Example 2, except that the amounts of the components of the surface treatment liquid were as shown in Table 2 below.
[0061] Table 2 Comparative composition and addition amount of the surface treatment solution provided in Preparation Examples 1-8
[0062]
[0063] Preparation Example 10-18
[0064] Preparation Examples 10-18 each provide a surface treatment solution.
[0065] Comparative Preparation Examples 1-8 were prepared according to the method of Preparation Example 2, except that the type and ratio of the silicone resin in the surface treatment solution are shown in Table 3 below.
[0066] Table 3 Types and ratios of silicone resins in the surface treatment solutions provided in Preparation Examples 10-18
[0067] Preparation Example Types and ratios of silicone resins 3 Amino silicone resin 10 Epoxy modified silicone resin 11 Polyester modified silicone resin 12 Amino silicone resin: epoxy modified silicone resin = 1:0.25 13 Amino silicone resin: epoxy modified silicone resin = 1:0.35 14 Amino silicone resin: epoxy modified silicone resin = 1:0.5 15 Amino silicone resin: epoxy modified silicone resin = 1: 0.75 16 Amino silicone resin: epoxy modified silicone resin = 1:0.9 17 Amino silicone resin: acrylic modified silicone resin = 1:0.5 18 Amino silicone resin: polyester modified silicone resin = 1:0.5
[0068] Examples 1-18
[0069] Examples 1-18 respectively provide a mica tube, and the difference between the above mica tubes is that the surface treatment liquid on the mica tube is derived from Preparation Examples 1-18 respectively.
[0070] The preparation method of the above mica tube is:
[0071] (1) Preparation of mica tube preform:
[0072] (1-1) Preparation of mica slurry: 75 g of mica powder, 50 g of polyethylene, 55 g of silica powder and 25 g of organic silica gel were mixed evenly, and stirred at a stirring speed of 700 r / min for 100 min to obtain mica slurry.
[0073] (1-2) Extrusion molding: The mica slurry is extruded at an extrusion temperature of 180°C, and then air-cooled at 25°C for 20 minutes to obtain a mica tube preform;
[0074] (2) Then, a surface treatment liquid is applied to the surface of the mica tube preform, and the coating amount of the surface treatment liquid is 35 g / m 2 .
[0075] (3) Drying: A double-stage drying process is used for drying. The first stage is dried at 90°C for 10 min. The second stage is dried at 160°C for 15 min to obtain a mica tube. The inner diameter of the mica tube is 10 mm, the outer diameter is 14 mm, and the thickness of the ceramic coating formed by the surface treatment liquid on the surface of the mica tube is 0.2 mm ± 0.03 mm.
[0076] Embodiment 19
[0077] Example 19 provides a mica tube.
[0078] Example 19 was carried out according to the method of Example 3, except that: in the preparation method of the mica tube of Example 19: the first stage drying temperature was 80°C, and the drying time was 10 min; the second stage drying temperature was 170°C, and the drying time was 15 min.
[0079] Embodiment 20
[0080] Example 20 provides a mica tube.
[0081] Example 20 was carried out according to the method of Example 3, except that: in the preparation method of the mica tube of Example 20: the first stage drying temperature was 100°C, and the drying time was 10 min; the second stage drying temperature was 150°C, and the drying time was 15 min.
[0082] Comparative Examples 1-8
[0083] Comparative Examples 1-8 each provide a mica tube.
[0084] Comparative Examples 1-8 were carried out according to the method of Example 3, except that the surface treatment liquids on the mica tubes of Comparative Examples 1-8 were derived from Comparative Preparation Examples 1-8, respectively.
[0085] Comparative Example 9
[0086] Comparative Example 9 provides a mica tube.
[0087] Comparative Example 9 was carried out according to the method of Example 3, except that: in the preparation method of the mica tube provided in Comparative Example 9, the drying temperature in one stage was 110° C. and the drying time was 5 min.
[0088] Comparative Example 10
[0089] Comparative Example 10 provides a mica tube.
[0090] Comparative Example 10 was carried out according to the method of Example 3, except that: in the preparation method of the mica tube provided in Comparative Example 10, the second-stage drying temperature was 140° C. and the time was 8 minutes.
[0091] Comparative Example 11
[0092] Comparative Example 11 provides a mica tube.
[0093] Comparative Example 11 was prepared according to the method of Example 3, except that: in the preparation method of the mica tube provided in Comparative Example 11, the second-stage drying temperature was 180° C. and the time was 8 min.
[0094] Performance testing
[0095] The physical properties and performance of the mica tubes obtained in Examples 1-20 and Comparative Examples 1-11 of the present application were tested, and the results are shown in Table 4.
[0096] (1) Physical properties: including whether the surface of the mica tube is uniform and flat, and whether cracks and powdering occur when burned at 600°C. Note: When the surface properties of the mica tube are not good, the fire resistance and voltage resistance related performance tests are directly abandoned, which is indicated by " / " in Table 4.
[0097] (2) A copper tube conductor is lined inside a mica tube and a copper wire is wound around the outside of the mica tube to obtain a test sample; then the test sample is subjected to a room temperature withstand voltage and fire resistance test;
[0098] ① Withstand voltage at room temperature: Place the test sample in a muffle furnace and set the temperature to 25°C; then gradually pressurize the conductor until the mica tube breaks down. The pressure at the time of breakdown is the normal withstand voltage.
[0099] ② Fire resistance: Place the test sample in a muffle furnace and pressurize the conductor to 25kV; then gradually increase the temperature until the mica tube breaks down. The temperature at the time of breakdown is the fire resistance temperature.
[0100] Table 4 Performance test results of mica tubes of Examples 1-20 and Comparative Examples 1-11
[0101]
[0102]
[0103] According to the test results in Table 4, the mica tubes provided in Examples 1-20 of the present application have a smooth surface, no cracks, and no powder loss, and the mica tubes have a withstand voltage of ≥55kv at room temperature and a fire resistance temperature of >900°C. This indicates that the mica tubes have excellent fire resistance and high temperature insulation, and can fully meet the use requirements of the insulation layer of the electrode rod or the out-of-bounds waterproof casing.
[0104] Although the mica tube obtained in Comparative Example 1 has a smooth surface, no cracks, and no powder falling, the insulation of the mica tube is slightly poor due to the small amount of ceramic powder added in the surface treatment liquid.
[0105] In Comparative Example 2, due to excessive addition of ceramic powder, powder falling off occurred on the surface of the mica tube.
[0106] In Comparative Example 3, since the amount of silicon dioxide added is too small, the uniformity of the surface treatment liquid is poor, and the vitrified coating formed on the surface of the mica tube is uneven, which ultimately leads to poor fire resistance and insulation of the mica tube.
[0107] In Comparative Example 4, due to excessive addition of silicon dioxide, the surface of the mica tube was rough and accompanied by powder falling.
[0108] In Comparative Example 5, since no glass powder was added to the surface treatment liquid, the vitrified coating on the surface of the mica tube fell off at high temperature.
[0109] In Comparative Example 6, due to excessive addition of glass powder, the surface of the mica tube is uneven, and the fire resistance and high-temperature insulation of the mica tube are poor.
[0110] In Comparative Example 7, since the amount of organic silicone resin added is too small, the organic silicone resin cannot fill the surface of the mica tube, so the surface of the mica tube is rough and uneven.
[0111] In Comparative Example 8, due to excessive addition of the organic silicone resin, the surface treatment liquid is too viscous, and thus the surface treatment liquid cannot form a vitrified coating on the surface of the mica tube.
[0112] In Comparative Example 9, in the double-stage drying process of the mica tube, the drying temperature of one stage was too high, resulting in bubbles appearing on the surface of the mica tube and poor surface properties of the mica tube.
[0113] In Comparative Example 10, since the drying temperature in the second stage is too low, the surface treatment liquid cannot be solidified, and it is difficult to form a vitrified coating on the surface of the mica tube.
[0114] In Comparative Example 11, in the double-stage drying process of the mica tube, the second-stage drying temperature is too high, resulting in bubbles appearing on the surface of the mica tube and poor surface performance of the mica tube.
[0115] From the test results of Examples 1-9, it can be seen that the application controls the addition amount of each component of the surface treatment liquid within the following range: 15-25 parts of ceramic powder, 35-55 parts of silicon dioxide, 5-15 parts of glass powder, and 35-45 parts of amino silicone resin. The obtained mica tube has a smooth surface, no cracks at high temperatures, and no powder falling. After performance testing, the room temperature withstand voltage of the above mica tube is 55-32kv / mm, and the fire resistance temperature is 939-972°C, indicating that the mica tube has excellent fire resistance and electrical insulation properties.
[0116] The test results of Example 3 and Examples 10-18 show that the fire resistance of the mica tubes of Examples 12-16 is better than that of the mica tubes of Examples 1, 10-11, and 17-18. This indicates that the fire resistance of the surface treatment liquid prepared by using a mixture of amino silicone resin and epoxy modified silicone resin is better than that of the surface treatment liquid prepared by using only one silicone resin or using amino silicone resin and acrylic modified silicone resin / polyester modified silicone resin. Further comparison shows that in Examples 13-15, the weight ratio of amino silicone resin to epoxy modified silicone resin is controlled between 1: (0.35-0.75), and the fire resistance temperature of the mica tube obtained can reach above 1000°C, and its fire resistance is even better.
[0117] It can be seen from the test results of Examples 3 and 19-20 that in the drying process of the mica tube preparation method of Examples 3 and 19-20, the first-stage drying temperature is controlled between 80-100°C, and the second-stage drying temperature is controlled between 150-170°C. The obtained mica tube has a smooth surface, no cracks, no powder falling, and excellent fire resistance and electrical insulation.
[0118] In summary, the mica tube provided in the present application is seamless and has a smooth surface. It has no cracks and no powder falling at a high temperature of 600°C. In addition, the performance test results show that the room temperature withstand voltage of the above-mentioned mica tube is ≥35kv and the fire resistance temperature is >900°C, which means that the above-mentioned mica tube has excellent fire resistance and high-temperature insulation, and can fully meet the use requirements of the insulation layer of the electrode rod or the out-of-bounds waterproof casing.
[0119] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A surface treatment liquid, characterized in that: The surface treatment liquid comprises the following components in parts by weight: 15-25 parts of ceramic powder, 35-55 parts of silicon dioxide, 5-15 parts of glass powder and 35-45 parts of organic silicon resin; The organic silicone resin is a mixture of an amino organic silicone resin and an epoxy modified organic silicone resin, and the weight ratio of the amino organic silicone resin to the epoxy modified organic silicone resin is 1:(0.35-0.75).
2. The surface treatment liquid according to claim 1, characterized in that: The surface treatment liquid comprises the following components in parts by weight: 20 parts of ceramic powder, 40 parts of silicon dioxide, 10 parts of glass powder and 40 parts of organic silicon resin.
3. A mica tube, characterized in that: The outer surface of the mica tube comprises a ceramic coating formed by the surface treatment liquid according to any one of claims 1 to 2.
4. The mica tube according to claim 3, characterized in that: The thickness of the porcelainizable coating is 0.2±0.03 mm.
5. The method for preparing a mica tube according to any one of claims 3 to 4, characterized in that: The following steps are involved: Preparation, coating and drying of mica tube preforms; The drying adopts a double-stage drying process; the first-stage drying temperature is 80-100° C., and the drying time is ≥8 minutes; the second-stage drying temperature is 150-170° C., and the drying time is ≥10 minutes.
6. The method for preparing a mica tube according to claim 5, characterized in that: In the coating step, the coating amount of the surface treatment liquid is 33-38 g / m 2 .