A rollable flexible crystalline silicon component and manufacturing method
By using laser cutting and low-temperature welding technology to form a curlable flexible crystal silicon module, the problem that existing photovoltaic modules cannot adapt to the curved surface is solved, and the effect of efficient power generation and lightweight portability is achieved.
Patent Information
- Application Number
- CN202311196636.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-14
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-09-14
AI Technical Summary
Most existing photovoltaic modules are unable to adapt to surfaces of different shapes, such as curved walls and building exterior walls, resulting in low power generation efficiency.
Using the method of making a curlable flexible crystal silicon component, by setting a dividing line on the cell and cutting it into small pieces with laser, metal wires plated with low temperature solder form an array, and laminated welding to form a curlable component, and filling it with acrylic powder coating. Cracks to achieve flexibility and efficient power generation of components.
It realizes efficient power generation that adapts to surfaces with different shapes, and the components are lightweight, easy to carry, and have rich color choices.
Smart Images

Figure CN117153943B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photovoltaics, and in particular relates to a rollable flexible crystalline silicon component and a manufacturing method thereof. Background Art
[0002] After the 1970s, with the development of modern industry, the global energy crisis and air pollution problems have become increasingly prominent. Traditional fuel energy is decreasing day by day, and the harm to the environment is becoming increasingly prominent. At the same time, about 2 billion people in the world do not have access to normal energy supply. At this time, the world has turned its attention to renewable energy, hoping that renewable energy can change the energy structure of mankind and maintain long-term sustainable development.
[0003] Solar energy has become the focus of attention due to its unique advantages. The abundant solar radiation energy is an important energy source, which is inexhaustible, pollution-free, cheap, and freely available to humans. The energy of solar energy reaching the ground every second is as high as 800 megawatt-hours. If 0.1% of the solar energy on the earth's surface is converted into electrical energy, with a conversion rate of 5%, the annual power generation can reach 5.6×1012 kilowatt-hours, which is equivalent to 40 times the world's energy consumption. It is precisely because of these unique advantages of solar energy that after the 1980s, the types of solar cells have continued to increase, the scope of application has become increasingly broad, and the market scale has gradually expanded.
[0004] Most of the current photovoltaic modules cannot be curled and cannot adapt to surfaces of different shapes, such as curved walls, building exteriors, etc., and their power generation efficiency is low. Summary of the invention
[0005] In view of this, the present invention provides a rollable flexible crystalline silicon component that can adapt to surfaces of different shapes, such as curved walls, building exterior walls, roof surfaces, etc., has high power generation efficiency, is light in weight, and is easy to carry.
[0006] The details are as follows:
[0007] A method for manufacturing a rollable flexible crystalline silicon component, the method comprising the following steps:
[0008] S1. Setting a dividing line on the battery cell;
[0009] S2, cutting the battery cell into N small battery strings along the dividing line by laser cutting without splitting, where N is a positive integer greater than or equal to 2;
[0010] S3, arranging metal wires with low-temperature solder plated on their surfaces in parallel into an array, wherein an adhesive film is disposed on the upper surface of the array;
[0011] S4, placing the lower surface of the array vertically on the silver grid line on the surface of the battery cell;
[0012] S5. Melt the low-temperature solder of the metal wire by lamination, and weld the low-temperature solder to the silver grid wire on the surface of the battery cell to form a rollable flexible crystalline silicon component.
[0013] Furthermore, a method for manufacturing a rollable flexible crystalline silicon component comprises:
[0014] After S2, acrylic powder coating is applied on the dividing line.
[0015] Furthermore, the method for manufacturing a rollable flexible crystalline silicon component includes: the lamination temperature is 140-155°C.
[0016] Furthermore, a method for manufacturing a rollable flexible crystalline silicon component comprises:
[0017] After S5, the minimum radius for rolling up the rollable flexible crystalline silicon component is R, and R decreases as N increases.
[0018] On the other hand, a rollable flexible crystalline silicon component is prepared by the above-mentioned method for preparing a rollable flexible crystalline silicon component.
[0019] Beneficial effects:
[0020] The present invention provides a rollable flexible crystalline silicon component that can adapt to surfaces of different shapes, such as curved walls, building exterior walls, roof surfaces, etc. It has high power generation efficiency, is light in weight, is easy to carry, and has rich colors. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of a method for manufacturing a rollable flexible crystalline silicon component in an embodiment of the present invention; DETAILED DESCRIPTION
[0022] The exemplary embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0023] like Figure 1 As shown, a method for manufacturing a rollable flexible crystalline silicon component comprises the following steps:
[0024] S1. Setting a dividing line on the battery cell;
[0025] S2, cutting the battery cell into N small battery strings along the dividing line by laser cutting without splitting, where N is a positive integer greater than or equal to 2;
[0026] S3, arranging metal wires with low-temperature solder plated on their surfaces in parallel into an array, and placing an adhesive film on the upper surface of the array for fixing;
[0027] The adhesive film is used to fix the array to prevent the position of the metal wire from changing during lamination.
[0028] S4, placing the lower surface of the array vertically on the silver grid line on the surface of the battery cell;
[0029] S5. Melt the low-temperature solder of the metal wire by lamination, and weld the low-temperature solder to the silver grid wire on the surface of the battery cell to form a rollable flexible crystalline silicon component.
[0030] Preferably, the cutting can be performed by an equal division method.
[0031] The metal wire is a wire with good conductive properties, including but not limited to: copper and aluminum.
[0032] The cell is a solar cell.
[0033] The silver grid lines are formed by silver paste plated on the main grid lines on the battery cell.
[0034] The array is used to collect current on the silver grid lines.
[0035] Furthermore, a method for manufacturing a rollable flexible crystalline silicon component comprises:
[0036] After S2, acrylic powder coating is applied on the dividing line.
[0037] Its function is to fill the cracks that may appear in the battery cells after cutting, enhance the flexibility of the battery cells, and increase the service life of the components.
[0038] Furthermore, the method for manufacturing a rollable flexible crystalline silicon component includes: the lamination temperature is 140-155°C.
[0039] Furthermore, a method for manufacturing a rollable flexible crystalline silicon component comprises:
[0040] After S5, the minimum radius for rolling up the rollable flexible crystalline silicon component is R, and R decreases as N increases.
[0041] It should be noted that the value of N can be set according to the minimum radius R of the component to be curled. If the component needs to be curled to a greater extent, the value of N needs to be set to a larger value.
[0042] The acrylic powder coating comprises an auxiliary agent, a curing agent and acrylic resin.
[0043] Furthermore, the weight portion of the curing agent accounts for 10 to 18% of the weight portion of the acrylic powder coating, and the curing agent includes a mixture of any one or more of the following: GMA acrylic acid, hydrogenated epoxy, carboxyl polyester, undecane dioic acid, sebacic acid, trimellitic anhydride, phthalic anhydride, and blocked isocyanate.
[0044] Further, the auxiliary agent accounts for 5-40% of the weight of the acrylic powder coating, and the auxiliary agent is a mixture of any one or more of the following: silicon dioxide, aluminum oxide, hindered amines, salicylate derivatives, benzophenone, thiodipropionate diester, hindered phenol, a mixture of ethylene oxide and propylene oxide, distearylethylenediamine, melamine formaldehyde resin, urea-formaldehyde resin, phenolic resin, acrylic acid, amide-modified phenol urea surfactant, polyolefin wax, polyamide wax. Of course, those skilled in the art can select other types of auxiliary agents according to actual needs, and the embodiments of the present invention will not be described in detail.
[0045] In the embodiment of the present invention, the refractive index of the acrylic resin is in the range of 1.40-1.50, preferably 1.42-1.48.
[0046] On the other hand, a rollable flexible crystalline silicon component is prepared by the above-mentioned method for preparing a rollable flexible crystalline silicon component.
[0047] Beneficial effects:
[0048] The present invention provides a rollable flexible crystalline silicon component and a manufacturing method, which can adapt to surfaces of different shapes, such as curved walls, building exterior walls, roof surfaces, etc., has high power generation efficiency, is light in weight, is easy to carry, and has rich colors.
[0049] Those skilled in the art will readily appreciate that the above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, combinations, replacements, improvements, etc. made within the spirit and principles of the present invention are included within the protection scope of the present invention.
Claims
1. A method for manufacturing a rollable flexible crystalline silicon component, characterized in that: The method comprises the following steps: S1. Setting a dividing line on the battery cell; S2, cutting the battery cell into N small battery strings along the dividing line by laser cutting without splitting, where N is a positive integer greater than or equal to 2; After S2, applying acrylic powder coating on the dividing line; S3, arranging metal wires with low-temperature solder plated on their surfaces in parallel into an array, and placing an adhesive film on the upper surface of the array for fixing; S4, vertically placing the lower surface of the array on the silver grid line on the surface of the battery cell; S5. Melt the low-temperature solder of the metal wire by lamination, and weld the low-temperature solder to the silver grid wire on the surface of the battery cell to form a rollable flexible crystalline silicon component.
2. The method for manufacturing a rollable flexible crystalline silicon component according to claim 1, characterized in that: The metal wires include: copper wires and silver wires.
3. The method for manufacturing a rollable flexible crystalline silicon component according to claim 1, characterized in that: The lamination temperature is 140-155°C.
4. The method for manufacturing a rollable flexible crystalline silicon component according to claim 1, characterized in that: include: After S5, the minimum radius for rolling up the rollable flexible crystalline silicon component is R, and R decreases as N increases.
5. The method for manufacturing a rollable flexible crystalline silicon component according to claim 1, characterized in that: The acrylic powder coating comprises an auxiliary agent, a curing agent and acrylic resin.
6. A rollable flexible crystalline silicon component, characterized in that: The rollable flexible crystalline silicon component is prepared by the manufacturing method of any one of claims 1 to 5.