A water-resistant carbon quantum dot-based composite phosphorescent material and preparation method thereof

Through the hydrothermal reaction of carbon source and urea, water-resistant carbon quantum dot-based composite phosphorescent materials are prepared, which solves the problems of short lifespan and deactivation of phosphorescent materials in water environment, and achieves the effect of maintaining phosphorescent properties underwater.

CN117165289BActive Publication Date: 2024-10-29TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311010009.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-10-29
Estimated Expiration
2043-08-11

AI Technical Summary

Technical Problem

Existing phosphorescent materials have short lifespans and are easily deactivated in a water environment, which limits the further development of their applications.

Method used

A water-resistant carbon quantum dot-based composite phosphorescent material is prepared by using a hydrothermal reaction between a carbon source and urea. The material maintains phosphorescent properties in an aqueous environment, does not contain metal elements, has low toxicity, and has a simple preparation process.

Benefits of technology

The phosphorescent material has an extended phosphorescent lifetime, maintains stable phosphorescent emission performance in an underwater environment, and has good water resistance and low toxicity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117165289B_ABST
    Figure CN117165289B_ABST
Patent Text Reader

Abstract

The present invention provides a water-resistant carbon quantum dot-based composite phosphorescent material and a preparation method thereof, belonging to the technical field of phosphorescent luminescent materials. The preparation method comprises: mixing a carbon source with urea, performing a hydrothermal reaction, and collecting a solid after the reaction is completed, which is a water-resistant carbon quantum dot-based composite phosphorescent material. The carbon source is a compound obtained by replacing at least one hydrogen atom on a benzene ring with a boric acid group and a chromophoric group, preferably 3-aminophenylboronic acid. The water-resistant carbon quantum dot-based composite phosphorescent material prepared by the method can produce blue phosphorescence for about 40 seconds after irradiation with ultraviolet light of 275nm, and the life span can reach more than 2s, and cyanuric acid crystals are formed on the surface of the carbon dot material, which can suppress the molecular vibration of the carbon dot, and effectively isolate the quenching of dissolved oxygen in water, so as to maintain good phosphorescence performance in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of phosphorescent materials, and in particular relates to a water-resistant carbon quantum dot-based composite phosphorescent material and a preparation method thereof. Background Art

[0002] Room temperature phosphorescent materials have unique advantages in bio-imaging, anti-counterfeiting and information encryption, light-emitting devices and other application fields due to their special optical properties of emitting long afterglow after excitation stops. However, most traditional room temperature phosphorescent materials are pure organic or doped with heavy metal atoms, so they always have disadvantages such as toxicity, complex preparation process and high cost. In addition, most phosphorescent materials are easily quenched by dissolved oxygen and solvent-assisted relaxation in aqueous solution. Most RTP materials can only exert phosphorescent properties under anhydrous solid conditions.

[0003] Compared with traditional room temperature phosphorescent materials, carbon dots not only have the characteristics of high biocompatibility, low toxicity, easy preparation, low cost, but also have excellent optical properties, so they are ideal materials for room temperature phosphorescent research. Carbon dots refer to zero-dimensional carbon nanomaterials with a size less than 10nm, most of which have sp 2 The lattice spacing of the hybrid carbon skeleton structure is consistent with that of graphite or amorphous carbon. The surface of carbon dots contains rich surface states, which can show bright visible fluorescence and afterglow under the excitation of light of a specific wavelength. Carbon dots have the advantages of good chemical stability, adjustable luminescence color, high fluorescence quantum yield, and resistance to photobleaching. They also have the characteristics of low toxicity, environmental protection, a wide range of carbon sources, and low preparation cost. However, existing phosphorescent carbon dot materials have problems such as short lifespan and phosphorescence quenching in water environment, which hinders further research and application of room temperature phosphorescent materials.

[0004] Therefore, it is necessary to provide an improved technical solution to address the above-mentioned deficiencies in the prior art. Summary of the invention

[0005] The purpose of the present invention is to provide a water-resistant carbon quantum dot-based composite phosphorescent material and a preparation method thereof. The method has simple steps and can prepare a composite phosphorescent material with a long phosphorescence lifetime and good water resistance, so as to solve the problems of the existing phosphorescent materials having a short lifetime and phosphorescence quenching in a water environment.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a water-resistant carbon quantum dot-based composite phosphorescent material comprises the following steps: mixing a carbon source with urea, carrying out a hydrothermal reaction, and collecting a solid after the reaction is completed to obtain the water-resistant carbon quantum dot-based composite phosphorescent material.

[0008] Preferably, the carbon source is a compound containing a benzene ring, and at least one hydrogen atom on the benzene ring is substituted by a boric acid group.

[0009] Preferably, the carbon source is a compound containing a benzene ring, and 1 to 2 hydrogen atoms on the benzene ring are substituted by boric acid groups.

[0010] Preferably, the carbon source is a compound containing a benzene ring, and 2 to 4 hydrogen atoms on the benzene ring are independently substituted by amino groups or carboxyl groups.

[0011] Preferably, the mixed solution of the carbon source and urea is placed in a heating device and reacted at 190-220° C. for 3-5 hours.

[0012] Preferably, the carbon source comprises at least one of 3-aminophenylboronic acid, phenylboronic acid, 1,3-phenylenediboronic acid, 2-aminophenylboronic acid, 4-aminophenylboronic acid and 4-carboxyphenylboronic acid.

[0013] Preferably, the mixed solution of the carbon source and urea is poured into an open container, and then the container opening is covered with a metal foil, and the container is placed in a heating device for reaction.

[0014] Preferably, the mass ratio of carbon source to urea is (0.020-0.100):3.

[0015] Preferably, the mass ratio of carbon source to urea is 0.025:3, and the reaction time is 3 hours.

[0016] The present invention also provides a water-resistant carbon quantum dot-based composite phosphorescent material, which is prepared by any of the above methods.

[0017] Beneficial effects:

[0018] (1) The phosphorescent carbon quantum dot-based composite material of the present invention is a solid carbon quantum dot-based composite material, which can maintain phosphorescent properties in an aqueous environment, does not contain metal elements, has low toxicity, and has a simple preparation process.

[0019] (2) The initial product of the solid-state carbon quantum dot-based composite material prepared by the present invention is a crystalline solid, which becomes a white powder after grinding. Under irradiation with 275nm excitation light, the emission peak of the product is located near 448nm, and it can emit blue phosphorescence, and the phosphorescence lifetime can reach more than 2s.

[0020] (3) The preparation of the solid carbon quantum dot-based composite material of the present invention is carried out under normal pressure hydrothermal conditions, the reaction time is short, the reaction conditions are easy to achieve, and the preparation process is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:

[0022] Figure 1 Actual pictures of the u-CDs provided in Example 1 of the present invention under the irradiation of a fluorescent lamp, a 365nm ultraviolet lamp, and after irradiation of a 365nm ultraviolet lamp.

[0023] Figure 2 Phosphorescence emission spectra of u-CDs provided in Example 1 of the present invention at different excitation wavelengths.

[0024] Figure 3 The fluorescence emission spectra of the u-CDs provided in Example 1 of the present invention at different excitation wavelengths.

[0025] Figure 4 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 1 of the present invention.

[0026] Figure 5 This is the XRD spectrum of u-CDs provided in Example 1 of the present invention.

[0027] Figure 6 This is a photo of phosphorescence emission of the u-CDs provided in Example 1 of the present invention after being excited by 254nm and 365nm excitation light in a water-immersed state.

[0028] Figure 7 This is the FT-IR spectrum of u-CDs provided in Example 1 of the present invention.

[0029] Figure 8 The phosphorescence emission spectrum of the u-CDs provided in Example 2 of the present invention at the optimal excitation wavelength.

[0030] Fig. 9 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 2 of the present invention.

[0031] Fig.10 The phosphorescence emission spectrum of the u-CDs provided in Example 3 of the present invention at the optimal excitation wavelength.

[0032] Fig.11 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 3 of the present invention.

[0033] Fig.12 The phosphorescence emission spectrum of the u-CDs provided in Example 4 of the present invention at the optimal excitation wavelength.

[0034] Fig.13 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 4 of the present invention.

[0035] Fig.14 The phosphorescence emission spectrum of the u-CDs provided in Example 5 of the present invention at the optimal excitation wavelength.

[0036] Fig.15 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 5 of the present invention.

[0037] Fig.16 The phosphorescence emission spectrum of the u-CDs provided in Example 6 of the present invention at the optimal excitation wavelength.

[0038] Fig.17 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 6 of the present invention.

[0039] Fig.18 The phosphorescence emission spectrum of the u-CDs provided in Example 7 of the present invention at the optimal excitation wavelength.

[0040] Fig.19 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 7 of the present invention.

[0041] Fig. 20 The phosphorescence emission spectrum of the u-CDs provided in Example 8 of the present invention at the optimal excitation wavelength.

[0042] Fig.21 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 8 of the present invention.

[0043] Fig. 22 The phosphorescence emission spectrum of the u-CDs provided in Example 9 of the present invention at the optimal excitation wavelength.

[0044] Fig.23 This is the room temperature phosphorescence decay spectrum of u-CDs provided in Example 9 of the present invention. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0046] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.

[0047] The present invention aims to solve the problems of short phosphorescence lifetime and water resistance of current phosphorescent materials, and provides a water-resistant carbon quantum dot-based composite phosphorescent material. The preparation method of the material is simple and easy to promote. The material has a long phosphorescence lifetime and good water resistance, and can still emit phosphorescence normally in an underwater environment.

[0048] The preparation method of the water-resistant carbon quantum dot-based composite phosphorescent material comprises the following steps: mixing a carbon source with urea, performing a hydrothermal reaction, and collecting a solid after the reaction is completed, which is the water-resistant carbon quantum dot-based composite phosphorescent material.

[0049] In a preferred embodiment of the present invention, the carbon source is a compound containing a benzene ring, and at least one (eg, two, three, four, five, six) hydrogen atoms on the benzene ring are substituted by a boric acid group.

[0050] In a preferred embodiment of the present invention, the carbon source is a compound containing a benzene ring, and 1 to 2 hydrogen atoms on the benzene ring are replaced by boric acid groups.

[0051] In a preferred embodiment of the present invention, the carbon source is a compound containing a benzene ring, and 2 to 4 hydrogen atoms on the benzene ring are independently substituted by amino groups or carboxyl groups.

[0052] In a preferred embodiment of the present invention, a mixed solution of the carbon source and urea is placed in a heating device and reacted at 190-220°C (e.g., 191°C, 195°C, 200°C, 205°C, 210°C, 215°C, 219°C) for 3-5h (e.g., 3.5h, 4.0h, 4.5h).

[0053] In a preferred embodiment of the present invention, the carbon source includes at least one of 3-aminophenylboronic acid, phenylboronic acid, 1,3-phenylenediboronic acid, 2-aminophenylboronic acid, 4-aminophenylboronic acid and 4-carboxyphenylboronic acid.

[0054] In a preferred embodiment of the present invention, a mixed solution of the carbon source and urea is poured into an open container, and then the container opening is covered with a metal foil, and the container is placed in a heating device for reaction.

[0055] In a preferred embodiment of the present invention, the mass ratio of the carbon source to urea is (0.020-0.100):3, for example, 0.021:3, 0.025:3, 0.030:3, 0.040:3, 0.050:3, 0.060:3, 0.070:3, 0.080:3, 0.090:3, and 0.099:3.

[0056] In a preferred embodiment of the present invention, the mass ratio of carbon source to urea is 0.025:3, and the reaction time is 3 hours.

[0057] The present invention also provides a water-resistant carbon quantum dot-based composite phosphorescent material, which is prepared by any of the above methods.

[0058] The following is a detailed description of a water-resistant carbon quantum dot-based composite phosphorescent material and a preparation method thereof according to the present invention through specific embodiments.

[0059] The sources of the following raw materials are as follows:

[0060] 3-Aminophenylboronic acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0061] Urea: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0062] 2-Aminophenylboronic acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0063] 4-Aminophenylboronic acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0064] 3-Carboxyphenylboronic acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0065] 4-Carboxyphenylboronic acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0066] Phenylboric acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.;

[0067] 1,3-Benzenediboric acid: analytical grade, purchased from Shanghai Titan Technology Co., Ltd.

[0068] In the following examples, the phosphorescence lifetime of u-CDs is calculated by the following formula:

[0069]

[0070] In the formula, τ avg is the phosphorescence lifetime of u-CDs, α i is the exponential factor, τ i is the life span, α i , τ i The lifetime curve is obtained by fitting the room temperature phosphorescence decay spectrum of the sample. In the present invention, Origin software is used to perform the relevant fitting process, and other software with the same function can also be used for processing.

[0071] Example 1

[0072] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0073] (1) Add 25 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0074] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 200 °C for 3 h.

[0075] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0076] like Figure 1 As shown, the u-CDs powder prepared in this embodiment is irradiated with a fluorescent lamp and a 365nm ultraviolet lamp respectively. It can be seen that the u-CDs powder is a white solid powder under sunlight (left figure), and under 365nm ultraviolet lamp, the u-CDs powder emits bright blue fluorescence (in the figure). After the 365nm ultraviolet lamp is turned off, the u-CDs powder emits bright cyan phosphorescence (right figure).

[0077] Figure 2 The phosphorescence emission spectra of the u-CDs powder prepared in this example at different excitation wavelengths are shown in the figure. The optimal excitation wavelength for the phosphorescence emission of u-CDs is 275 nm, and the corresponding emission peak is 448 nm, which can produce blue phosphorescence.

[0078] Figure 3 The fluorescence emission spectra of the u-CDs powder prepared in this example at different excitation wavelengths are shown in the figure. The optimal excitation wavelength for the fluorescence emission of the u-CDs prepared in this example is 260 nm, and the corresponding emission peak is 340 nm.

[0079] Figure 4 This is the phosphorescence decay spectrum of the u-CDs powder prepared in this example. It can be seen that the afterglow lasts for about 40 seconds. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.351s.

[0080] Figure 5 XRD diffraction spectra of u-CDs and cyanuric acid prepared in this embodiment. As shown in the figure, cyanuric acid crystals exist in the u-CDs powder material prepared in this embodiment, and the crystalline rigid network formed by cyanuric acid can not only effectively inhibit the molecular vibration of carbon dots and reduce non-radiative transitions, but also the carbon dots can effectively isolate the quenching of dissolved oxygen in water under the coating of cyanuric acid, so that u-CDs can maintain its phosphorescence performance in an aqueous environment.

[0081] The u-CDs powder prepared in this example was mixed with water in a test tube and excited using excitation light with wavelengths of 254 nm and 365 nm, respectively. Figure 6 As shown, after the u-CDs powder prepared in this embodiment is immersed in water, it is excited by an excitation light with a wavelength of 254nm, which can produce blue phosphorescence, and it is excited by an excitation light with a wavelength of 365nm, which can produce cyan phosphorescence, proving that the u-CDs powder prepared in this embodiment has good water resistance.

[0082] In addition, different solutions with a pH value of 0 to 14 were used instead of water for immersion. When the immersion lasted for more than one week, the luminescent materials were excited with excitation light of wavelengths of 254 nm and 365 nm, and good phosphorescence performance was still maintained.

[0083] Figure 7 The FT-IR spectrum of the u-CDs powder prepared in this example is shown in the figure. The FT-IR spectrum of the u-CDs powder has the following wavelengths at wave numbers of 3000-3200, 1722, 1463, and 1398 cm -1 Obvious peaks appear at the 400 nm, corresponding to functional groups such as NH, C=O, CN, and C=N.

[0084] Example 2

[0085] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0086] (1) Add 50 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0087] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 200 °C for 3 h.

[0088] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0089] Figure 8 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 447 nm, which can produce blue phosphorescence.

[0090] Fig. 9 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration is more than 35s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τi 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.276s.

[0091] Example 3

[0092] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0093] (1) Add 100 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0094] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 200 °C for 3 h.

[0095] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0096] Fig.10 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 447 nm, which can produce blue phosphorescence.

[0097] Fig.11 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration is more than 35s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.187s.

[0098] By comparing the phosphorescence emission spectra and phosphorescence lifetime decay spectra of Examples 1 to 3, it can be found that with the increase of the carbon source doping amount, the phosphorescence intensity and phosphorescence lifetime of the u-CDs sample both show a downward trend.

[0099] Example 4

[0100] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0101] (1) Add 25 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0102] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 190 °C for 4 h.

[0103] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0104] Fig.12 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak of the u-CDs prepared in this example is 448 nm, which can produce blue phosphorescence.

[0105] Fig.13 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow lasts for about 40 seconds. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.364s.

[0106] Example 5

[0107] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0108] (1) 100 mg of 3-aminophenylboronic acid was added to 3 g of urea, and the mixture was dissolved and mixed evenly with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0109] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 190 °C for 4 h.

[0110] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0111] Fig.14 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 449 nm.

[0112] Fig.15This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration is close to 40s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.259s.

[0113] Example 6

[0114] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0115] (1) 25 mg of 3-aminophenylboronic acid was added to 3 g of urea, and the mixture was dissolved and mixed evenly with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0116] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 210 °C for 3 h.

[0117] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0118] Fig.16 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 447 nm.

[0119] Fig.17 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration is more than 35s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.229s.

[0120] Example 7

[0121] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0122] (1) Add 25 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0123] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 220 °C for 3 h.

[0124] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0125] Fig.18 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 448 nm.

[0126] Fig.19 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration reaches 40s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.307s.

[0127] Example 8

[0128] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0129] (1) Add 25 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0130] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 200 °C for 4 h.

[0131] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0132] Fig. 20 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 448 nm.

[0133] Fig.21 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration reaches 40s. After fitting with a three-exponential function, according to the formula τ avg=Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.300s.

[0134] Example 9

[0135] This embodiment provides a water-resistant carbon quantum dot-based composite phosphorescent material, and the preparation method thereof is as follows:

[0136] (1) Add 25 mg of 3-aminophenylboronic acid to 3 g of urea, dissolve and mix well with 20 mL of deionized water to obtain a mixed solution of 3-aminophenylboronic acid and urea.

[0137] (2) The mixed solution was placed in a 100 mL beaker, covered with tin foil to prevent the solution from evaporating too quickly, and placed in an oven for hydrothermal reaction at 200 °C for 5 h.

[0138] (3) After the reaction is completed, the mixture is cooled to room temperature, the solid in the beaker is taken out, and ground into powder using a mortar to obtain a water-resistant carbon quantum dot-based composite phosphorescent material, referred to as u-CDs.

[0139] Fig. 22 This is the phosphorescence emission spectrum of the u-CDs prepared in this example at an excitation wavelength of 275 nm. As shown in the figure, the emission peak position of the u-CDs prepared in this example is 448 nm.

[0140] Fig.23 This is the phosphorescence decay spectrum of the u-CDs prepared in this example. It can be seen from the figure that the afterglow duration is close to 40s. After fitting with a three-exponential function, according to the formula τ avg =Σα i τ i 2 / α i τ i , the calculated phosphorescence lifetime of u-CDs is 2.241s.

[0141] Embodiments 10 to 14

[0142] On the basis of Example 1, phenylboronic acid, 2-aminophenylboronic acid, 4-aminophenylboronic acid, 1,3-phenylenediboronic acid, and 4-carboxyphenylboronic acid were used instead of 3-aminophenylboronic acid, and other conditions remained unchanged to prepare u-CDs, and their optimal excitation wavelength and emission peak position were analyzed as follows:

[0143] Example Carbon source Optimal excitation wavelength / nm Emission peak position / nm 10 Phenylboronic acid 270 408 11 2-Aminophenylboronic acid 260 431 12 4-Aminophenylboronic acid 280 465 13 1,3-phenylenediboronic acid 260 444 14 4-Carboxyphenylboronic acid 260 423

[0144] Under the above excitation conditions, phenylboronic acid, 2-aminophenylboronic acid, 4-aminophenylboronic acid, and 1,3-phenylenediboronic acid can emit phosphorescence visible to the naked eye, but the duration is short, and the calculated phosphorescence lifetime is also shorter than that of 3-aminophenylboronic acid.

[0145] Comparative Example 1

[0146] On the basis of Example 1, the tin foil placed on the mouth of the beaker was removed, and other conditions remained unchanged to prepare u-CDs. During the reaction, the water was quickly evaporated within half an hour, and the target product could not be obtained.

[0147] Comparative Example 2

[0148] On the basis of Example 1, the amount of 3-aminophenylboronic acid was adjusted to 10 mg, and other conditions remained unchanged to prepare u-CDs, whose optimal excitation wavelength was 275 nm, emission peak position was 447 nm, and phosphorescence lifetime was 2.259 s.

[0149] Comparative Example 3

[0150] On the basis of Example 1, the amount of 3-aminophenylboronic acid was adjusted to 150 mg, and other conditions remained unchanged to prepare u-CDs, whose optimal excitation wavelength was 275 nm, emission peak position was 445 nm, and phosphorescence lifetime was 2.017 s.

[0151] In summary, the phosphorescent carbon quantum dot-based composite materials prepared in the present invention can realize the emission of blue phosphorescence, and the phosphorescent carbon quantum dot-based composite materials prepared in the present invention have very stable material properties under different preparation conditions and carbon source doping amounts, and the emission wavelength and phosphorescence lifetime are stable. The preparation conditions are simple and it is easy to meet the conditions for mass production.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a water-resistant carbon quantum dot-based composite phosphorescent material, characterized in that: The method comprises the following steps: mixing a carbon source with urea, carrying out a hydrothermal reaction, and collecting a solid after the reaction is completed, which is a water-resistant carbon quantum dot-based composite phosphorescent material; The carbon source is at least one of 3-aminophenylboronic acid, phenylboronic acid, 1,3-phenylenediboronic acid, 2-aminophenylboronic acid, 4-aminophenylboronic acid and 4-carboxyphenylboronic acid; The temperature of the hydrothermal reaction is 190-220° C., and the reaction time is 3-5 hours.

2. The method for preparing a water-resistant carbon quantum dot-based composite phosphorescent material according to claim 1, characterized in that: The mixed solution of the carbon source and urea is poured into an open container, and then the container mouth is covered with metal foil, and the container is placed in a heating device for reaction.

3. The method for preparing a water-resistant carbon quantum dot-based composite phosphorescent material according to claim 2, characterized in that: The mass ratio of carbon source to urea is (0.020~0.100):

3.

4. The method for preparing a water-resistant carbon quantum dot-based composite phosphorescent material according to claim 3, characterized in that: The mass ratio of carbon source to urea was 0.025:3, and the reaction time was 3 h.

5. A water-resistant carbon quantum dot-based composite phosphorescent material, characterized in that: The method is prepared by the method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Room-temperature phosphorescent carbon dot material and preparation method and application thereof

    CN110205121A

  • Phosphorescent carbon dot-metal organic framework composite material as well as preparation method and application thereof

    CN114381261A

  • Preparation and application of water and heating continuous stimulation response phosphorescent carbon quantum dots

    CN114540017A

  • Blue-purple phosphorescent carbon quantum dots and preparation method thereof

    CN115197699A