Super-strain and self-adhesive flexible hydrogel as well as preparation method and application thereof

By extracting nanocellulose and polysaccharide compounds from wheat straw and acrylamide monomers, a flexible cellulose hydrogel with superstrain and strong adhesion, the tensile strain range of traditional hydrogel sensors is solved. The problems of narrowness and low adhesion have achieved the application prospects in human movement health monitoring and self-driven power supply.

CN118955953AInactive Publication Date: 2024-11-15GUANGDONG UNIV OF TECH

Patent Information

Application Number
CN202411290076.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing hydrogel sensors have narrow tensile strain range and low adhesion, making it difficult to meet the needs of high mechanical performance and multifunctional applications.

Method used

By extracting nanocellulose from wheat straw, combining acrylamide monomers and polysaccharide compounds, the polymerization reaction conditions are controlled, and flexible cellulose hydrogel with superstrain and strong adhesion is formed, enhancing its mechanical properties and electrical conductivity, and enhancing its mechanical properties and electrical conductivity. .

Benefits of technology

The super-strain tensile range and strong adhesion of the hydrogel are realized, expanding its prospects for human sports health monitoring and self-driven power supply applications, and meeting the actual needs of wearable strain electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955953A_ABST
    Figure CN118955953A_ABST
Patent Text Reader

Abstract

The invention discloses super-strain and self-adhesive flexible hydrogel as well as a preparation method and application thereof. The invention relates to a preparation method of flexible cellulose hydrogel, which comprises the following steps: (1) performing sodium hydroxide alkali treatment and tetramethylpiperidine oxide and sodium hypochlorite oxidation treatment on wheat straw, cleaning and centrifuging to obtain wheat straw nano cellulose; (2) adding water into the wheat straw nanocellulose to obtain a nanocellulose suspension, then adding an acrylamide monomer, a polysaccharide compound, an initiator and a cross-linking agent, and stirring to obtain a uniform mixed solution; and (3) pouring the mixed solution into a mold, and heating to obtain the nanocellulose composite hydrogel. The hydrogel prepared by the invention has a super-strain tensile range and strong adhesion, and a sensor prepared from the flexible hydrogel has excellent sensing capability in the aspect of human motion health monitoring, so that the application prospect of the hydrogel sensor is effectively expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of cellulose hydrogel materials, and in particular to a super-strained, self-adhesive flexible hydrogel and a preparation method and application thereof. Background Art

[0002] With the rapid development of artificial intelligence technology and market demand, flexible smart wearable devices have attracted widespread research interest in recent years. Flexible strain hydrogel sensors are similar to soft electronic skins as an important candidate material for wearable devices. After being subjected to external forces, hydrogel sensors can quickly detect the stress state and instantaneous deformation of hydrogels through real-time resistance change signals, and can also be used for green energy collection and self-driven power supply applications. In order to meet the application requirements of different scenarios, hydrogel sensors, in addition to the necessary mechanical strength, conductivity, and responsiveness, must also have super strain stretching range and strong adhesion to adapt to multifunctionality and different application scenarios. Generally speaking, the tensile strain capacity of hydrogels depends on the physical hydrogen bonds, van der Waals forces, and chemical covalent bonds between polymer chains. When hydrogels are subjected to external forces, the energy dissipation process accompanied by the continuous breaking and reorganization of single or multiple physical and chemical bonds is considered to be conducive to achieving super strain and strong adhesion. However, traditional hydrogel strain sensors usually have a narrow tensile strain range and low adhesion. Hydrogels are easily damaged by external stretching or bending forces, resulting in poor sensing ability and adhesion performance, which greatly limits its sensing application.

[0003] CN117050337A discloses a self-healing, self-adhesive and strain-sensitive ion-conductive hydrogel, which utilizes a hydrogen peroxide-ascorbic acid redox system to initiate copolymerization of N-isopropylacrylamide and acrylic acid and Al 3+ The hydrogel has a self-healing, stretchable and self-adhesive properties by complexing and crosslinking with -COOH, but the tensile strain of the hydrogel is 600% and the tensile fracture strength is 3kPa, which cannot meet the use requirements of high mechanical performance hydrogel sensors. CN116655954A discloses an adhesive self-healing organic hydrogel, which improves the mechanical properties of the hydrogel by forming a physically crosslinked poly(N-[tris(hydroxymethyl)methyl]acrylamide-co-acrylamide) network in the presence of cellulose nanofibers, metal salts and polyols. The tensile strain is 1333.50%, the tensile strength is 290.02kPa, and the adhesion is 1.52g. The tensile strain range and adhesion capacity are limited. Therefore, the preparation of a hydrogel with super strain and strong adhesion has become a problem to be solved. Summary of the invention

[0004] In order to solve the existing technical problems, the present invention provides a super-strain, self-adhesive flexible hydrogel and its preparation method and application. The prepared hydrogel has a super-strain stretching range and strong adhesion, and the flexible hydrogel has excellent sensing ability in human sports health monitoring, effectively expanding the application prospects of hydrogel sensors. Furthermore, nanocellulose of different sizes can be obtained by designing different extraction processes, controlling the mass ratio of nanocellulose to water and the polymerization reaction conditions of acrylamide monomers and different types of polysaccharide compounds, and effectively regulating the mechanical properties of the obtained hydrogel, and further assembling a flexible hydrogel sensor.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] The first aspect of the present invention provides a method for preparing a flexible cellulose hydrogel, comprising the following steps:

[0007] (1) wheat straw is treated with sodium hydroxide and oxidized with tetramethyl piperidine oxide and sodium hypochlorite, and then washed and centrifuged to obtain wheat straw nanocellulose;

[0008] (2) adding water to the wheat straw nanocellulose to obtain a nanocellulose suspension, and then adding acrylamide monomers, polysaccharide compounds, initiators, and cross-linking agents, and stirring to obtain a uniform mixed solution;

[0009] (3) pouring the mixed solution into a mold and heating it to obtain a nanocellulose composite hydrogel.

[0010] Preferably, step (1) specifically comprises the following steps: treating the wheat straw with 5-15wt% sodium hydroxide solution at 78-85°C for 30-60min, then washing with deionized water until neutral, then oxidizing with 1-10wt% tetramethylpiperidinium oxide and sodium hypochlorite for 30-60min, and finally washing and centrifuging to obtain wheat straw nanocellulose.

[0011] Preferably, in step (1), the length of the wheat straw nanocellulose is 30-145 μm, and the diameter is 62±3 nm; when the length distribution percentage of the wheat straw nanocellulose reaches 50%, the corresponding length is 90±5 μm.

[0012] Preferably, in step (2), the mass ratio of the wheat straw nanocellulose to water is 1:(10-50).

[0013] Preferably, in step (2), the mass ratio of the wheat straw nanocellulose to the acrylamide monomer is 1:(5-8); in a preferred embodiment of the present invention, in step (2), the mass ratio of the wheat straw nanocellulose to the acrylamide monomer is 1:8.

[0014] Preferably, in step (2), the mass ratio of the acrylamide monomer to the polysaccharide compound is 1:(0.3-1); in a preferred embodiment of the present invention, in step (2), the mass ratio of the acrylamide monomer to the polysaccharide compound is 1:(0.5-0.6).

[0015] Preferably, the acrylamide monomer includes at least one of methacrylamide, acrylamide, N-butylacrylamide, N-ethylacrylamide, N-hydroxyacrylamide, N-phenylacrylamide, N-tert-butylacrylamide and N-hydroxyethylacrylamide; further preferably, the acrylamide monomer includes at least one of acrylamide and methacrylamide.

[0016] Preferably, the polysaccharide compound includes at least one of laminarin, curdlan, lichenin, fucoidan, yeast polysaccharide, lentinan, astragalus polysaccharide, pullulan, hydroxyethyl deacetylated chitosan, chitin, lactose N-fucoidan V, maltodextrin, and erucic acid acyl-β-D-glucoside; further preferably, the polysaccharide compound includes at least one of laminarin and pullulan.

[0017] Preferably, the initiator includes at least one of 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, benzoyl peroxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, ammonium persulfate, azobisimidazolinepropane, potassium persulfate, 2,2'-azabis(2-imidazoline) dihydrochloride, and isooctyl p-dimethylaminobenzoate; further preferably, the initiator includes at least one of ammonium persulfate and potassium persulfate.

[0018] Preferably, the crosslinking agent includes at least one of 3,3'-dithiodipropionic acid di(N-hydroxysuccinimide) ester, glutaraldehyde, 3-methyl-2-thiazolidinethione, 4-maleimidobutyric acid-N-succinimide ester, dimethyl pimelimidate dihydrochloride, 1,4-bis[(glycidyloxy)methyl]cyclohexane, N,N'-methylenebisacrylamide, N-tert-butyloxycarbonyl-2-(2-aminoethoxy)ethylamine, epichlorohydrin, hexamethylenebisacrylamide, and N,N'-(1,2-dihydroxyethylene)diacrylamide; further preferably, the crosslinking agent includes at least one of epichlorohydrin and N,N'-methylenebisacrylamide.

[0019] Preferably, in step (3), the heating temperature is 20-80° C. and the heating time is 1-24 h.

[0020] The second aspect of the present invention provides a flexible cellulose hydrogel prepared by the flexible cellulose hydrogel preparation method.

[0021] The third aspect of the present invention provides the use of the flexible cellulose hydrogel in the preparation of flexible cellulose hydrogel sensors and friction nanogenerators.

[0022] A fourth aspect of the present invention provides a flexible cellulose hydrogel sensor, the structure of which includes the flexible cellulose hydrogel and copper electrodes and wires connected at both ends thereof.

[0023] A fifth aspect of the present invention provides a friction nanogenerator, the structure of which includes VBH tape, copper foil, a hydrogel layer, a Kapton film, and silica gel; the hydrogel layer is the flexible cellulose hydrogel.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention extracts nanocellulose from wheat straw, which has excellent linearity and mechanical strength. Nanocellulose of different sizes can be obtained by designing different extraction processes, and the mass ratio of nanocellulose to water and the polymerization reaction conditions of acrylamide monomers and different types of polysaccharides are controlled to effectively regulate the mechanical properties of the prepared hydrogel. The prepared flexible cellulose hydrogel has super strain and strong adhesion, and has good application prospects in strain sensing and human motion health detection. In addition, the assembled friction nanogenerator sensor can self-drive to collect green energy, which can be used for self-driven power supply of small electronic devices, which well meets the practical application requirements in the field of wearable strain electronic devices.

[0026] 2. As a reinforcing agent, wheat straw nanocellulose has excellent hydrophilic hydroxyl groups and rigidity, and can bend and entangle with the polymer skeleton to form physical or chemical synergy, which helps to enhance the tensile strength and toughness of the hydrogel cross-linked network and improve the tensile strain range and adhesion of the hydrogel sensor.

[0027] 3. The present invention uses polysaccharide compounds, which form chemical covalent bonds under the action of cross-linking agents, and have a double cross-linked network structure with both physical and chemical bonds, which effectively improves the cross-linked network tension of the hydrogel. The prior art also uses other polysaccharide substances, such as glucose, but it has been found through experiments that the structure of polysaccharides has an impact on the performance of hydrogels. The fucoidan and lichen polysaccharide in the present invention are aliphatic compounds with stable six-membered ring structures, and pullulan is a compound with good linear molecular chains. Physical hydrogen bonds can be formed between polysaccharide chemicals and polyacrylamide molecular chains, especially pullulan with a linear molecular chain structure can be bent arbitrarily after combining with polyacrylamide molecular chains, and the cross-linked network with strong tension is conducive to enhancing the energy dissipation and reconstruction of the hydrogel during the process of being subjected to external forces.

[0028] 4. The wheat straw nanocellulose and laminarin or pullulan used in the present invention have the characteristics of natural green high-value utilization, and can effectively highlight the mechanical properties and conductive properties of the hydrogel sensor, thereby realizing its application in the field of strain sensing.

[0029] 5. The free radical polymerization initiation system used in the method of the present invention has the characteristics of low toxicity, simple operation and environmental protection.

[0030] 6. The process of the method of the present invention is simple and easy to scale up for production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The microscopic morphology of different nanocelluloses in Example 1;

[0032] Figure 2 The microscopic morphology structure diagram of the hydrogel prepared in Example 1-8;

[0033] Figure 3 1 is the tensile stress-strain curve of the hydrogel of the embodiment and the comparative example;

[0034] Figure 4 The resistance response diagram of the hydrogel prepared in Example 4 under different tensile strains (0-1000%) (a) and the resistance response stability curve of 1000s cyclic loading-unloading under a tensile strain of 50% (b);

[0035] Figure 5 The flexible wearable hydrogel strain sensor of Example 4 is used for health monitoring of different joint movements of the human body;

[0036] Figure 6 The flexible hydrogel triboelectric nanogenerator sensor assembled for Examples 1-8 is tested for its power generation capability, and is used to power LED lights of small electronic devices to achieve self-driven collection of green energy;

[0037] Figure 7 The flexible friction nanogenerator insole assembled with the hydrogel in Example 4 monitors different motion states. DETAILED DESCRIPTION

[0038] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0039] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0040] Example 1

[0041] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0042] (1) Extraction of nanocellulose:

[0043] 10.0 g of wheat straw was treated with 100 g of 5% sodium hydroxide at 80° C. for 60 min, then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 1% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 60 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted; number S1;

[0044] 10.0 g of wheat straw was treated with 100 g of 5% sodium hydroxide at 80° C. for 60 min, then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 5% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 60 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted; number S2;

[0045] 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 5% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted; number S3;

[0046] 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted; number S4;

[0047] 10.0 g of wheat straw was treated with 100 g of 15% sodium hydroxide at 80° C. for 60 min, then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 60 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted; number S5;

[0048] (2) 1.0 g of the above-mentioned nanocellulose S4 was dissolved in 10 g of water and ultrasonically treated for 10 min to form a uniformly dispersed transparent solution;

[0049] (3) then adding 5.0 g of methacrylamide and 1.5 g of laminarin to the above solution in sequence, stirring thoroughly to dissolve, then adding 0.022 g of potassium persulfate initiator and 0.003 g of epichlorohydrin crosslinker, stirring to obtain a fully dissolved mixed solution;

[0050] (4) pouring the mixed solution into a mold and reacting it under vacuum and a constant temperature of 40° C. for 24 hours;

[0051] (5) The prepared hydrogel is connected to a copper electrode and a wire to form a flexible cellulose hydrogel sensor.

[0052] Example 2

[0053] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0054] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0055] S2, dissolving 1.0 g of nanocellulose in 20 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0056] S3, then add 5.0g of methacrylamide and 2.0g of pullulan to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of ammonium persulfate initiator and 0.003g of epichlorohydrin cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0057] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 12 hours;

[0058] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0059] Example 3

[0060] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0061] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0062] S2, dissolving 1.0 g of nanocellulose in 30 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0063] S3, then add 5.0g of methacrylamide and 2.5g of pullulan to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of ammonium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0064] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 6 hours;

[0065] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible hydrogel sensor.

[0066] Example 4

[0067] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0068] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0069] S2, dissolving 1.0 g of nanocellulose in 40 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0070] S3, then add 8.0g of methacrylamide and 4.4g of pullulan to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0071] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 3 h;

[0072] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0073] Example 5

[0074] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0075] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0076] S2, dissolving 1.0 g of nanocellulose in 40 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0077] S3, then add 8.0g of methacrylamide and 4.4g of laminarin to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0078] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 3 h;

[0079] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0080] Example 6

[0081] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0082] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0083] S2, dissolving 1.0 g of nanocellulose in 40 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0084] S3, then add 8.0g of methacrylamide and 5.6g of laminarin to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0085] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 3 h;

[0086] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0087] Example 7

[0088] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0089] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0090] S2, dissolving 1.0 g of nanocellulose in 50 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0091] S3, then add 8.0g of methacrylamide and 5.6g of pullulan to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of epichlorohydrin cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0092] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 1 h;

[0093] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0094] Example 8

[0095] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0096] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0097] S2, dissolving 1.0 g of nanocellulose in 50 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0098] S3, then add 8.0g of methacrylamide and 5.6g of laminarin to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of epichlorohydrin cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0099] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 1 h;

[0100] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0101] The microstructure of the nanocellulose prepared in Example 1 is shown in FIG. Figure 1 As shown, Figures ae and e are respectively the images of S1-5 nanocellulose. Figure 2 ah are respectively the microscopic morphological structure diagrams of the hydrogels prepared in Examples 1-8.

[0102] Comparative Example 1

[0103] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0104] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0105] S2, dissolving 1.0 g of nanocellulose in 40 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0106] S3, then add 8.0g of methacrylamide and 4.4g of fucoidan to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0107] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 3 h;

[0108] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0109] Comparative Example 2

[0110] A super-strain, self-adhesive flexible cellulose hydrogel sensor and a preparation method thereof, comprising the following steps:

[0111] S1. 10.0 g of wheat straw was treated with 100 g of 10% sodium hydroxide at 80° C. for 30 min, and then washed with deionized water and centrifuged until the pH of the solution was neutral; the precipitate was oxidized with 2.0 g of 10% tetramethylpiperidinyl oxide and 6.2 g of sodium hypochlorite for 30 min, and after multiple washing and centrifugation, concentrated nanocellulose was extracted;

[0112] S2, dissolving 1.0 g of nanocellulose in 40 g of water, and ultrasonically treating for 10 min to form a uniformly dispersed transparent solution;

[0113] S3, then add 8.0g of methacrylamide and 4.4g of lichen polysaccharide to the above solution in sequence, stir thoroughly to dissolve, then add 0.022g of potassium persulfate initiator and 0.003g of N,N'-methylenebisacrylamide cross-linking agent, stir to obtain a fully dissolved mixed solution;

[0114] S4, pouring the mixed solution into a mold, and reacting it under vacuum and a constant temperature of 40° C. for 3 h;

[0115] S5. Connect the prepared hydrogel to the copper electrode and the wire to assemble into a flexible cellulose hydrogel sensor.

[0116] The particle size of the nanocellulose prepared in Example 1 is shown in Table 1 below.

[0117] Table 1

[0118] Experimental Case Length / μm Diameter / nm S1 10-70 100±3 S2 15-85 83±3 S3 20-120 75±3 S4 30-145 62±3 S5 30-80 55±3

[0119] From Table 1 and Figure 1 From the microscopic morphology, we can see that nanocellulose of different sizes has different line diameter ratios, which have different effects on the microstructure and conductive properties of the hydrogel. Figure 2 a and Figure 2 As can be seen from Figure b, the use of different types of polysaccharides in Examples 1-2 will result in significantly different pore structures of the hydrogels. The pullulan hydrogel structure of Example 2 has more and denser pores. Different ratios of polysaccharides are used in Examples 3 and 4, and the corresponding SEM images show that Figure 2 The hydrogel pores of d in the embodiment are larger and more uniform. The microstructures of the hydrogels using different proportions of laminarin are also different, where the corresponding Figure 2 The hydrogel microstructure of e showed more microporous and dense structure. Figure 2 g and Figure 2 As can be seen from the h in the figure, the microstructure of the hydrogel containing pullulan has more microporous structures and better uniformity. In short, the hydrogel prepared with nanocellulose S4 and pullulan has a larger network pore size and better uniformity, which is beneficial to improve the tensile strength of the hydrogel and improve the mechanical properties of the hydrogel.

[0120] The adhesion performance, mechanical performance and human motion sensing performance of the flexible cellulose hydrogel sensors prepared in Examples 1-8 were tested. The specific testing methods are as follows:

[0121] (1) Adhesion performance test of flexible cellulose hydrogel sensor

[0122] The hydrogel was made into a cubic strip (50 mm × 10 mm × 1 mm), and the hydrogel prepared in Examples 1-8 was bonded to the surface of the PVC material. The hydrogel and the surface of the PVC material were subjected to a 180° peeling test using a peeling force testing machine with a tensile rate of 50 mm / min, thereby obtaining different adhesion properties as shown in Table 2.

[0123] Table 2 Adhesion value of hydrogel prepared in Examples 1-8 to PVC material surface

[0124] Material gf / mm Example 1 2.84 Example 2 4.10 Example 3 5.13 Example 4 8.43 Example 5 6.15 Example 6 5.22 Example 7 4.86 Example 8 3.07 Comparative Example 1 2.91 Comparative Example 2 4.86

[0125] As can be seen from Table 2, the hydrogel prepared in Example 4 has the strongest adhesion to the PVC film. Compared with metal sensors, which have poor ductility and are difficult to bend or closely contact with non-planar objects, the hydrogel in Example 4 with strong adhesion ability helps to improve the accuracy and stability of sensor signal detection.

[0126] (2) Mechanical properties and human motion sensing performance testing of flexible cellulose hydrogel sensors

[0127] According to the hydrogel tensile test standard GB / T 16491-2008, the size of the hydrogel sample was designed to be length * width * height = 50mm * 10mm * 1mm, and the mechanical properties of the hydrogel were tested using a universal tensile testing machine with a tensile rate of 50mm / min. The test results are shown in Figure 3 .

[0128] Depend on Figure 3 It can be seen that the tensile strain and tensile strength of the hydrogels in the examples and comparative examples change with the changes in different polysaccharides and their dosages, wherein the tensile strain in Example 4 can reach 4335%, and the tensile strength reaches 1.24Mpa, indicating that the tensile strain of the hydrogel prepared in Example 4 is the largest. In general, the hydrogel prepared with pullulan in this example meets the requirements of the use scenario of the hydrogel sensor in the super strain tensile range.

[0129] The hydrogel prepared in Example 4 obtained the corresponding resistance change rate when the tensile strain was set to 10%, 20%, 50%, 100%, 200%, 500%, and 1000%. Figure 4 The resistance change rates obtained in a are 4%, 8%, 23%, 54%, 110%, 580%, and 2300%, respectively, indicating that the hydrogel prepared in Example 4 can quickly adapt to the sensing requirements under different strain conditions. At the same time, the hydrogel prepared in Example 4 was continuously loaded-unloaded for 1000s under 50% strain, and the load-unload cycle stretching resistance stability within 1000s was obtained. Figure 4 From b, we can see that the hydrogel sensor has excellent self-recovery ability and conductive anti-fatigue ability, and can achieve stable and reliable sensing signals.

[0130] Detection of different joint movements of the human body: In order to further explore the practicality of hydrogel sensors in flexible wearable electronic devices, the hydrogel prepared in Example 4 was integrated into the fingers, wrists, knees and throat for pronunciation testing. The response sensing signals of the subtle movements of different joints were detected by the resistance change of the digital source meter. Figure 5 As shown by Figure 5It can be seen that the hydrogel sensor can quickly and accurately capture the resistance change sensing signals corresponding to the subtle movements of different joints of the human body, indicating that the hydrogel sensor has good conductive sensing capabilities.

[0131] (3) Power supply performance test of flexible cellulose hydrogel friction nanogenerator sensor

[0132] The hydrogels of Examples 1-8 were made into cubic strips (50mm×10mm×1mm). Flexible friction nanogenerator sensors were assembled using VBH tape, kapton insulating material, copper foil, silica gel, and cellulose hydrogel. They were connected to a stepper and the sensor's power generation capacity was tested using an oscilloscope. The power generation device was connected to a small electronic device LED lamp to convert mechanical energy into electrical energy, which was self-powered for the LED lamp device, achieving effective collection and high-quality utilization of green energy.

[0133] from Figure 6 As can be seen from the figure, the flexible friction nanogenerator sensor prepared by Examples 1-8. Figure 3 , the mechanical properties of the hydrogel affect the hydrogel friction nano-power generation capacity. Under the same working conditions, the AC voltage generated by Example 4 can reach up to 20V. The hydrogel micro-network structure of Example 4 is larger in size and more uniform. The pore structure is conducive to the hydrogel to produce better mechanical strain adaptability and free electron migration. At the same time, it shows that wheat straw nanocellulose plays a good overlapping and conductive role between the cross-linked networks of the hydrogel. The hydrogel prepared in this example has good flexibility and conductivity, and can be used for the normal operation of self-powered LDE lamps. This provides an effective way to achieve green energy collection and utilization.

[0134] Figure 7 It is a flexible nano friction generator insole sensor assembled with the hydrogel sample of Example 4, which is used to monitor the electrical signals generated by the human body in slow, medium and fast motion states. As can be seen from the figure, the sensor can accurately and timely judge different motion states. This opens up an application mode for realizing human-computer interactive intelligent sensing applications. For example, it provides an accurate and scientific basis for judging physical rehabilitation exercises for disabled people, which is beneficial to generate electrical signal strength according to the sensor, and helps to realize rehabilitation applications in the field of human-computer interaction. In short, the flexible cellulose hydrogel sensor of the present invention has excellent superstrain and adhesion, as well as the ability of sensing conductivity and self-powered green energy collection, which can meet the application needs of multiple scenarios and has the application potential for manufacturing flexible wearable devices.

[0135] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A method for preparing a flexible cellulose hydrogel, characterized in that: The following steps are involved: (1) wheat straw is treated with sodium hydroxide and oxidized with tetramethyl piperidine oxide and sodium hypochlorite, and then washed and centrifuged to obtain wheat straw nanocellulose; (2) adding water to the wheat straw nanocellulose to obtain a nanocellulose suspension, and then adding acrylamide monomers, polysaccharide compounds, initiators, and cross-linking agents, and stirring to obtain a uniform mixed solution; (3) pouring the mixed solution into a mold and heating it to obtain a nanocellulose composite hydrogel.

2. The method for preparing the flexible cellulose hydrogel according to claim 1, characterized in that: In step (1), the length of the wheat straw nanocellulose is 30-145 μm and the diameter is 62±3 nm.

3. The method for preparing the flexible cellulose hydrogel according to claim 1, characterized in that: In step (2), the mass ratio of the wheat straw nanocellulose to water is 1:(10-50); the mass ratio of the wheat straw nanocellulose to acrylamide monomers is 1:(5-8), and the mass ratio of the acrylamide monomers to polysaccharides is 1:(0.3-1).

4. The method for preparing the flexible cellulose hydrogel according to claim 1, characterized in that: The acrylamide monomers include at least one of methacrylamide, acrylamide, N-butylacrylamide, N-ethylacrylamide, N-hydroxyacrylamide, N-phenylacrylamide, N-tert-butylacrylamide, and N-hydroxyethylacrylamide; the polysaccharide compounds include at least one of laminarin, curdlan, lichenin, fucoidan, yeast polysaccharide, lentinan, astragalus polysaccharide, pullulan, hydroxyethyl deacetylated chitosan, chitin, lactose N-fucoidan V, and maltodextrin.

5. The method for preparing the flexible cellulose hydrogel according to claim 1, characterized in that: The initiator includes at least one of 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, benzoyl peroxide, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, ammonium persulfate, azodiimidazole propane, potassium persulfate, 2,2'-azabis(2-imidazoline) dihydrochloride, and isooctyl p-dimethylaminobenzoate; the crosslinking agent includes 3,3'-dithiodipropionic acid di(N-hydroxybutyl) At least one of diimide) ester, glutaraldehyde, 3-methyl-2-thiazolidinethione, 4-maleimidobutyric acid-N-succinimide ester, dimethyl pimelimidate dihydrochloride, 1,4-bis[(glycidyloxy)methyl]cyclohexane, N,N′-methylenebisacrylamide, N-tert-butyloxycarbonyl-2-(2-aminoethoxy)ethylamine, epichlorohydrin, hexamethylenebisacrylamide, and N,N′-(1,2-dihydroxyethylene)diacrylamide.

6. The method for preparing the flexible cellulose hydrogel according to claim 1, characterized in that: In step (3), the heating temperature is 20-80°C and the heating time is 1-24h.

7. A flexible cellulose hydrogel, characterized in that The flexible cellulose hydrogel is prepared by the preparation method of any one of claims 1 to 6.

8. Use of the flexible cellulose hydrogel according to claim 7 in the preparation of flexible cellulose hydrogel sensors and friction nanogenerators.

9. A flexible cellulose hydrogel sensor, characterized in that: The structure of the flexible cellulose hydrogel sensor comprises the flexible cellulose hydrogel according to claim 7 and copper electrodes and wires connected at both ends thereof.

10. A friction nanogenerator, characterized in that: The structure of the friction nanogenerator includes VBH tape, copper foil, a hydrogel layer, a Kapton film, and silica gel; the hydrogel layer is the flexible cellulose hydrogel described in claim 7.

Citation Information

Patent Citations

  • Polyacrylamide / nano-crystalline cellulose high-strength dual-network composite gel preparation method

    CN107446144A

  • Preparation method of flexible strain sensor based on nanocellulose-carbon nanotube / polyacrylamide conductive hydrogel

    CN110183688A

  • Adhesive self-healing organic hydrogel sensor and preparation method thereof

    CN116655954A

Cited By

  • Honeycomb-like flexible sensor, preparation method and application in wearable device

    CN119573955A

  • Hydrogel-based super-tensile flexible multifunctional input device and preparation and application thereof

    CN119798515A

  • A hydrogel-based ultrastretchable flexible multifunctional input device and preparation and application thereof

    CN119798515B