A GeTe thin film material sample for TG-DSC test of LTCC and its preparation method

Through the GeTe film deposition technology after spin coating and exposure treatment, combined with the acetone solution stripping method, the problems of low utilization rate and low test efficiency of GeTe films in TG-DSC testing are solved, and efficient and accurate film sample preparation and test.

CN117214236BActive Publication Date: 2024-10-01JIANGSU FREETEL COMM CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311379439.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-23
Publication Date
2024-10-01
Estimated Expiration
2043-10-23

AI Technical Summary

Technical Problem

The GeTe thin film material has low utilization rate and low test efficiency in TG-DSC testing, mainly because the mechanical scraping method causes the film to adhere to the substrate or the substrate components are doped during the film collection process, and the heat absorption of the film cannot be accurately distinguished. exothermic peak.

Method used

The GeTe film was deposited on the substrate after spin-coating reverse photoresist, baking, exposure and development, and the GeTe film sample was obtained by acetone solution stripping method to avoid mechanical scraping and ensure that the film was completely separated from the substrate.

Benefits of technology

It improves the effective utilization rate and testing efficiency of the GeTe film, ensures the purity and integrity of the film, and can accurately measure its crystallization temperature and melting point temperature, significantly improving the accuracy and efficiency of the test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117214236B_ABST
    Figure CN117214236B_ABST
Patent Text Reader

Abstract

The present invention provides a GeTe thin film material sample for TG-DSC test of LTCC and a preparation method thereof. The preparation method of the GeTe thin film material sample comprises: (1) cleaning and baking a substrate to obtain a pre-treated substrate; (2) spin coating a reverse photoresist on the pre-treated substrate to obtain a composition of a substrate and a photoresist; (3) baking and exposing the composition of the substrate and the photoresist; (4) developing treatment; (5) depositing a GeTe thin film by magnetron sputtering to obtain a GeTe thin film substrate; (6) peeling the GeTe thin film substrate to obtain a GeTe thin film material sample. The GeTe thin film material sample prepared by the preparation method of the present invention can be completely detached from the substrate, avoiding the problem that a part of the thin film is attached to the substrate or the components of the substrate are doped in the tested thin film sample during the process of collecting the thin film, resulting in low effective utilization rate of the thin film and low test efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin film characterization sample preparation, and in particular relates to a GeTe thin film material sample for TG-DSC testing of LTCC and a preparation method thereof. Background Art

[0002] Many materials can be prepared in both amorphous and crystalline forms, but few have the unique combination of properties like phase-change materials in chalcogenides, including rapid crystallization of the amorphous phase, large optical and electrical contrast between the two phases, and high stability of the amorphous phase. These properties make them useful materials for data storage.

[0003] Phase change materials have been used by the optical storage industry for rewritable CDs and DVDs, using changes in their reflectivity to store information as light and dark areas. In recent years, non-volatile memories have also begun to use phase change materials, using corresponding changes in resistivity to achieve non-volatile information storage. For optical and electrical storage, to switch states, external heating pulses are required (laser pulses for optical storage and electrical pulses for electrical storage), and depending on the amplitude of the temperature rise and the cooling rate, a crystalline or amorphous phase will be formed. To form the amorphous phase, a DC pulse with a higher amplitude and a shorter time is required to raise the material temperature to the melting point temperature T m The atoms are cooled to an amorphous solid state and locked in their high resistance state by rapid quenching. To form a crystalline phase, a DC pulse with a slightly higher amplitude and a slightly longer duration is required to raise the temperature of the material above the crystallization temperature (T cry ) but kept below the melting point for a period of time, allowing the atoms to form a somewhat periodic arrangement, eventually forming a low resistance state.

[0004] Among phase change materials, germanium telluride (GeTe) has attracted more and more research attention due to its unique high crystallinity, high reliability, high on-state resistance ratio and low on-state resistivity. For GeTe materials, the properties of thin films are quite different from those of bulk materials. The crystallization temperature (T cry ) and melting point temperature (T m ) is the key to ensure the effectiveness of the device. The exothermic and endothermic temperature changes of the material are tested by the TG-DSC method, and the samples required for the test require intrinsic materials. Therefore, the film attached to the substrate needs to be separated from the substrate and placed in the crucible used in the experiment. The existing mechanical scraping method will cause part of the film to adhere to the substrate or the components of the substrate to be doped in the tested film sample during the process of collecting the film, resulting in low effective utilization of the film and the final test data cannot distinguish the intrinsic endothermic and exothermic peaks of the film, and the test efficiency is low. Summary of the invention

[0005] The problem to be solved by the present invention is to provide a GeTe thin film material sample for TG-DSC test of LTCC and a preparation method thereof, so as to solve the problem of low utilization rate and low test efficiency of the GeTe thin film material sample in TG-DSC test.

[0006] The technical solution adopted to solve the technical problem is to provide a method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC, comprising the following steps:

[0007] (1) cleaning and baking the substrate to obtain a pretreated substrate;

[0008] (2) spin coating a reverse photoresist on the pretreated substrate to obtain a composition of the substrate and the photoresist;

[0009] (3) baking and exposing the composition of substrate and photoresist;

[0010] (4) developing the composition of the substrate and the photoresist after the treatment in step (3);

[0011] (5) depositing a GeTe thin film on the developed substrate and the photoresist composition by magnetron sputtering to obtain a GeTe thin film substrate;

[0012] (6) The GeTe thin film substrate is peeled off to obtain a GeTe thin film material sample.

[0013] The beneficial effect of the technical solution adopted in the present invention is that the GeTe thin film material sample prepared by the above preparation method can be completely detached from the substrate, avoiding the adhesion of part of the thin film to the substrate or the components of the substrate being doped into the tested thin film sample during the process of collecting the thin film, thereby effectively solving the problems of low effective utilization rate of the thin film and low test efficiency.

[0014] Preferably, in step (1), the material of the substrate is high-resistance silicon, glass or sapphire; the cleaning is performed using the RCA standard cleaning method; the baking temperature is 110-130° C., and the baking time is 4.5-5.5 min.

[0015] The beneficial effect of the preferred technical solution adopted by the present invention is that the high-resistance silicon, glass or sapphire substrate has good bonding with the photoresist, and the photoresist can be evenly attached to the substrate.

[0016] Preferably, the reverse photoresist in step (2) is AZ5214 reverse photoresist, and the thickness of the reverse photoresist is 0.8 to 1.2 μm.

[0017] Preferably, the spin coating in step (2) includes primary spin coating and secondary spin coating; the primary spin coating speed is 900-1100 rpm, and the spin coating time is 8-12 s; the secondary spin coating speed is 2500-3500 rpm, and the spin coating time is 25-35 s.

[0018] Preferably, the baking and exposure in step (3) include the following steps: first baking at 90-110°C for 55-65s, then exposing the baked substrate and photoresist composition for a first time for 3-5s; then baking at 110-130°C for 80-100s, followed by a second exposure for 35-45s.

[0019] The beneficial effects of the preferred technical solution adopted in the present invention are as follows: the solvent in the photoresist can be partially volatilized by baking, the adhesion, light absorption and corrosion resistance of the photoresist can be enhanced, the stress generated in the photoresist film during the coating process can be alleviated, and the AZ5214 reverse photoresist can be denatured from a positive photoresist to a negative photoresist that is easy to peel off by performing a first exposure of 3 to 5 seconds and a second exposure of 35 to 45 seconds.

[0020] Preferably, no mask is used during the exposure process.

[0021] The beneficial effect of the preferred technical solution of the present invention is that no mask is used, and after the reverse photoresist is developed with a developer, all exposed areas are not dissolved, so the larger the area of ​​the photoresist, the larger the area of ​​the film that is peeled off.

[0022] Preferably, step (4) comprises the following steps: developing the substrate and photoresist composition after the secondary exposure for 30 seconds, then rinsing with deionized water and drying with nitrogen gas.

[0023] The beneficial effect of the preferred technical solution of the present invention is that after development, the photoresist is directly rinsed with deionized water and dried with nitrogen without post-baking, so that the photoresist is easier to remove.

[0024] Preferably, the stripping method in step (6) is: stripping by immersion in acetone solution.

[0025] Preferably, the thickness of the GeTe thin film material sample is 0.6-1 μm.

[0026] The beneficial effect of the preferred technical solution adopted in the present invention is: to ensure good test performance, the thickness of the GeTe thin film material sample used for TG-DSC test is not less than 0.6μm. The GeTe thin film material sample with a thickness exceeding 1μm is difficult to peel off and the film cannot be effectively detached smoothly.

[0027] The present invention also provides a GeTe thin film material sample prepared by the method for preparing the GeTe thin film material sample for TG-DSC testing of LTCC.

[0028] The present invention has the following beneficial effects:

[0029] (1) The present invention denatures the photoresist from positive photoresist to negative photoresist through secondary exposure, making it easier to peel off. The prepared GeTe thin film material sample shows high film utilization rate and test efficiency in TG-DSC test;

[0030] (2) The GeTe thin film material sample prepared by the present invention can be automatically separated from the substrate without the need for mechanical scraping, and the preparation efficiency is high;

[0031] (3) The GeTe thin film material samples prepared by the present invention have good uniformity, controllable film thickness, high purity and good integrity after peeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic flow chart of a method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC provided in an embodiment of the present invention;

[0033] Figure 2 It is a cross-sectional schematic diagram of the photolithography of the photoresist reverse glue, the deposition of the thin film and the thin film stripping process;

[0034] Figure 3 It is a temperature-pulse schematic diagram of the phase transition of sulfur compounds;

[0035] Figure 4 This is a TG-DSC test graph of the GeTe thin film material sample prepared by the present invention;

[0036] Figure 5 This is the TG-DSC test graph of the GeTe thin film sample prepared by mechanical exfoliation. DETAILED DESCRIPTION

[0037] The features and performance of the present invention are further described in detail below in conjunction with embodiments.

[0038] Example 1

[0039] A method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC comprises the following steps:

[0040] (1) The high-resistance silicon substrate is cleaned according to the RCA standard and baked at 120° C. for 5 minutes to obtain a pretreated substrate;

[0041] (2) placing the pretreated substrate on a coating table, dropping AZ5214 reverse glue on the pretreated substrate, spin coating at a rotation speed of 1000 rpm for 10 seconds, and then spin coating at a rotation speed of 3000 rpm for 30 seconds, so that the thickness of the photoresist on the pretreated substrate is 1 μm, and obtaining a composition of substrate and photoresist;

[0042] (3) placing the spin-coated substrate and photoresist composition on a heating table at 100° C. for baking for 60 seconds, then performing a first exposure for 4 seconds, then placing it on a heating table at 120° C. for baking for 90 seconds, and then performing a second exposure for 40 seconds;

[0043] (4) developing the substrate and photoresist composition after the secondary exposure for 30 seconds, then rinsing it three times with deionized water, and drying it with nitrogen gas;

[0044] (5) depositing a GeTe thin film on the developed substrate and the photoresist composition by magnetron sputtering, with a deposition thickness of 0.8 μm, to obtain a GeTe thin film substrate;

[0045] (6) Soak the GeTe thin film substrate in an acetone solution and wait for 5 minutes. The GeTe thin film material sample will fall off the substrate.

[0046] This embodiment also includes a GeTe thin film material sample for TG-DSC testing of LTCC.

[0047] Example 2

[0048] A method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC comprises the following steps:

[0049] (1) The glass substrate is cleaned according to the RCA standard and baked at 110° C. for 5.5 min to obtain a pretreated substrate;

[0050] (2) placing the pretreated substrate on a coating table, dropping AZ5214 reverse glue on the pretreated substrate, spin coating at a rotation speed of 900 rpm for 12 seconds, and then spin coating at a rotation speed of 2500 rpm for 35 seconds, so that the thickness of the photoresist on the pretreated substrate is 0.8 μm, and obtaining a composition of substrate and photoresist;

[0051] (3) placing the spin-coated substrate and photoresist composition on a heating table at 90° C. for baking for 65 seconds, then performing a first exposure for 3 seconds, then placing it on a heating table at 110° C. for baking for 100 seconds, and then performing a second exposure for 35 seconds;

[0052] (4) developing the substrate and photoresist composition after the secondary exposure for 30 seconds, then rinsing it three times with deionized water, and drying it with nitrogen gas;

[0053] (5) depositing a GeTe thin film on the developed substrate and the photoresist composition by magnetron sputtering, with a deposition thickness of 0.6 μm, to obtain a GeTe thin film substrate;

[0054] (6) Soak the GeTe thin film substrate in an acetone solution and wait for 5 minutes. The GeTe thin film material sample will fall off the substrate.

[0055] This embodiment also includes a GeTe thin film material sample for TG-DSC testing of LTCC.

[0056] Example 3

[0057] A method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC comprises the following steps:

[0058] (1) The sapphire substrate is cleaned according to the RCA standard and baked at 130° C. for 4.5 min to obtain a pretreated substrate;

[0059] (2) placing the pretreated substrate on a coating table, dropping AZ5214 reverse glue on the pretreated substrate, spin coating at a rotation speed of 1100 rpm for 8 seconds, and then spin coating at a rotation speed of 3500 rpm for 25 seconds, so that the thickness of the photoresist on the pretreated substrate is 1.2 μm, and obtaining a composition of substrate and photoresist;

[0060] (3) placing the spin-coated substrate and photoresist composition on a heating table at 110° C. for baking for 55 seconds, then performing a first exposure for 5 seconds, then placing it on a heating table at 130° C. for baking for 80 seconds, and then performing a second exposure for 45 seconds;

[0061] (4) developing the substrate and photoresist composition after the secondary exposure for 30 seconds, then rinsing it three times with deionized water, and drying it with nitrogen gas;

[0062] (5) depositing a GeTe thin film on the developed substrate and the photoresist composition by magnetron sputtering, with a deposition thickness of 1 μm, to obtain a GeTe thin film substrate;

[0063] (6) Soak the GeTe thin film substrate in an acetone solution and wait for 5 minutes. The GeTe thin film material sample will fall off the substrate.

[0064] This embodiment also includes a GeTe thin film material sample for TG-DSC testing of LTCC.

[0065] Comparative Example 1

[0066] A method for preparing a GeTe thin film material sample for TG-DSC testing of LTCC comprises the following steps:

[0067] (1) The high-resistance silicon substrate is cleaned according to the RCA standard and baked at 120° C. for 5 minutes to obtain a pretreated substrate;

[0068] (2) depositing a GeTe thin film on the pretreated substrate by magnetron sputtering, with a deposition thickness of 0.8 μm, to obtain a GeTe thin film substrate;

[0069] (3) Place the GeTe thin film substrate on a transparent tape, and peel it off to make it into a thinner layer of thin sheets. Then, peel the layer of thin sheets on the tape off into a crucible.

[0070] This embodiment also includes a GeTe thin film material sample for TG-DSC testing of LTCC.

[0071] Experimental example

[0072] Combination Figure 1 and Figure 2 It can be seen that Figure 1 The structure of the substrate and the photoresist reverse glue obtained by the microfabrication lithography process from the first step to the fourth step is as follows Figure 2 As shown in (a), since no mask is used in the process, the exposed area of ​​the photoresist reverse glue is not dissolved after being developed by the developer, so the larger the area of ​​the photoresist, the larger the area of ​​the film to be peeled off; the fifth step uses the magnetron sputtering method to Figure 2 (a) based on the deposition of GeTe thin film, as shown in Figure 2 (b) The substrate / photoresist / GeTe film structure, the temperature of the film deposition process should not be too high, too high temperature will lead to the failure of the photoresist, resulting in difficulty in subsequent stripping; in the sixth step, the substrate after the film deposition is placed in a container of a culture dish or flask containing an acetone solution. Due to the characteristics of the photoresist, after the solution is in an organic solvent such as acetone, the deposited film has no photoresist support and is broken into several small particles suspended in the solution, such as Figure 2 As shown in (c), the film is detached from the substrate, and then the sample that meets the TG-DSC test can be obtained by collecting and drying in a crucible.

[0073] Figure 3 This is a temperature-pulse diagram of the phase change of sulfur compounds. When a pulse higher than T is applied to the amorphous phase change material cry And lower than T m After the temperature pulse, the material changes from a disordered amorphous structure to an orderly crystalline structure, and the resistance changes from a high resistance state to a low resistance state; and when a rapid pulse exceeding T is applied to the crystalline phase change material, m And quickly quenched to Tcry After the temperature pulse, the ordered structure of the material is disrupted and there is no time to rearrange it in order, so it is locked in a disordered structure, and the resistance changes from a low resistance state to a high resistance state.

[0074] Figure 4 and Figure 5It can be seen that when the GeTe film is collected by scraping the substrate by mechanical stripping, there will always be a part of the film attached to the substrate or the components of the substrate are doped in the tested sample. The final test data is as follows Figure 5 As shown in FIG. 1 , the intrinsic endothermic and exothermic peaks of GeTe thin films cannot be distinguished; however, the method of the present invention can well solve these two shortcomings. The test data are shown in FIG. Figure 4 As shown in Figure 2, the exothermic peak at 195°C and the endothermic peak at 735°C are clearly found, which correspond exactly to the T of GeTe. cry and T m , it can be seen that the present invention has a great impact on the T of GeTe cry and T m The measurement is more accurate and has certain advantages over the traditional method of preparing test samples.

[0075] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any form. Any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the scope of the present invention.

Claims

1. A method for preparing GeTe thin film material samples for TG-DSC testing of LTCC, It is characterized in that The following steps are involved: (1) cleaning and baking the substrate to obtain a pretreated substrate; (2) spin coating a reverse photoresist on the pretreated substrate to obtain a composition of the substrate and the photoresist; (3) baking and exposing the composition of substrate and photoresist; (4) developing the substrate and photoresist composition after the treatment in step (3); (5) depositing a GeTe thin film on the developed substrate and the photoresist composition by magnetron sputtering to obtain a GeTe thin film substrate; (6) peeling off the GeTe thin film substrate to obtain a GeTe thin film material sample; The reverse photoresist in step (2) is AZ5214 reverse photoresist, and the thickness of the reverse photoresist is 0.8-1.2 μm; the spin coating in step (2) includes primary spin coating and secondary spin coating; the primary spin coating speed is 900-1100 rpm, and the spin coating time is 8-12 s; the secondary spin coating speed is 2500-3500 rpm, and the spin coating time is 25-35 s; The baking and exposure in step (3) include the following steps: first baking at 90-110° C. for 55-65 seconds, then exposing the baked substrate and photoresist composition for a first time for 3-5 seconds; then baking at 110-130° C. for 80-100 seconds, then exposing for a second time for 35-45 seconds; no mask is used during the exposure process; The step (4) comprises the following steps: developing the substrate and photoresist composition after the secondary exposure for 30 seconds, then washing with deionized water and drying with nitrogen gas; The GeTe thin film material sample has a thickness of 0.6-1 μm.

2. The preparation method according to claim 1, Features: In the step (1), the material of the substrate is high-resistance silicon, glass or sapphire; the cleaning is carried out by the RCA standard cleaning method; the baking temperature is 110-130° C., and the baking time is 4.5-5.5 min.

3. The preparation method according to claim 1, It is characterized in that The stripping method in step (6) is: stripping by immersion in acetone solution.