A processing method for hydrophilic and hydrophobic composite texture micro-grinding head and a bone micro-grinding device

Through the processing method of hydrophilic and hydrophilic composite texture micro-grinding head, the problems of the bonding strength between abrasive particles and substrate and the low utilization rate of cooling media are solved, and efficient cooling media aggregation and transportation are achieved, improving the cooling effect and grinding performance.

CN117257390BActive Publication Date: 2024-11-15QINGDAO UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310944648.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-28
Publication Date
2024-11-15
Estimated Expiration
2043-07-28

AI Technical Summary

Technical Problem

The existing micro-grinding head preparation process cannot effectively solve the problems of bonding strength between abrasive particles and substrate and the utilization rate of cooling media, resulting in poor cooling effect.

Method used

The hydrophilic composite textured micro-grinding head processing method is adopted to form alternatingly distributed hydrophilic stripes through substrate surface pretreatment, abrasive hydrophilization, orderly arrangement, double electroplating and deposition, acid etching treatment and laser etching technology. Enhance the hydrophobic properties of the plating and improve the aggregation and transportation efficiency of the cooling medium.

Benefits of technology

It significantly improves the aggregation speed and utilization rate of the cooling medium, reduces the residence time of the droplets on the surface of the coating, enhances the cooling effect, reduces the grinding temperature, and extends the service life of the micro-grinding head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117257390B_ABST
    Figure CN117257390B_ABST
Patent Text Reader

Abstract

The invention discloses a method for processing a hydrophilic-hydrophobic composite texture micro-grinding head and a bone micro-grinding device, which relates to the technical field of grinding head processing, pre-treating the surface of the micro-grinding head substrate to roughen the substrate surface; heat-treating the diamond abrasive grains to make the abrasive grains hydrophilic; using a dispensing machine to evenly dispense glue on the substrate surface, sprinkling the abrasive grains on the substrate surface, so that the abrasive grains are orderly arranged on the substrate surface; placing the substrate with the abrasive grains in a deposition liquid, using a constant voltage DC power supply for primary deposition; then in a deposition liquid with the same composition and the same temperature, increasing the current density for secondary deposition; acid-etching the substrate after the secondary deposition at a set temperature, so that the coating on the substrate surface forms a hydrophobic surface; using laser etching technology to form hydrophilic stripes on the hydrophobic surface, so that the hydrophilic stripes and the hydrophobic stripes are alternately distributed. The invention can increase the adsorption capacity of the cooling medium and improve the cooling effect of the cooling medium.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grinding head processing, and in particular to a processing method of a hydrophilic-hydrophobic composite texture micro-grinding head and a bone micro-grinding device. Background Art

[0002] Bone grinding is an important part of neurosurgery. In surgeries such as brain tumor resection, femoral necrosis, and bone cancer, high-speed rotating micro-grinding heads are used to grind and remove bones. Compared with other grinding methods, bone grinding is an energy-intensive operation process. Most of the grinding power is converted into heat, which is transferred from the grinding area to the bone tissue, the grinding head, the cooling medium, and the bone chips. In order to solve the problem of high-temperature thermal damage during grinding, there are currently some bone micro-grinding devices, such as:

[0003] CN115044950A discloses a bionic desert beetle self-transport bone micro-grinding head and its preparation process, the preparation process of which is as follows: selecting diamond abrasive grains and oxidizing the diamond abrasive grains; scanning the surface of a substrate by laser to form a hydrophobic substrate; or obtaining a hydrophobic coating by a chemical modification method; combining the oxidized diamond abrasive grains with the hydrophobic substrate or the hydrophobic coating by electroplating to obtain a micro-grinding head capable of capturing cooling medium droplets.

[0004] CN107789031A discloses a handheld neurosurgery rotary ultrasonic resonance water-collecting grinding device, comprising a main shaft, which is arranged in an electric spindle housing, a rotor winding is arranged on the outer circumference of the main shaft, and a stator winding corresponding to the rotor winding is arranged in the electric spindle housing, and the stator winding can be energized to drive the main shaft to rotate; a water-collecting abrasive tool for grinding biological bones, the main shaft is connected to the water-collecting abrasive tool through an ultrasonic vibration mechanism, and driven by the main shaft and the ultrasonic vibration mechanism, the water-collecting abrasive tool realizes longitudinal vibration and rotational motion, and micro-convex bodies are arranged on the surface of the water-collecting abrasive tool.

[0005] CN208065229U discloses a medical micro bone grinding tool with orderly arranged abrasive particles, which is divided into two parts: a working part, a cutter head, and a clamping handle. The working part is composed of a cutter head base, diamond abrasive particles, and a brazing metal binder. The cutter head of the working part is a micro sphere, and the diamond abrasive particles arranged thereon are orderly arranged.

[0006] Through research, it is found that although the existing micro-grinding head preparation process can achieve orderly arrangement of abrasive grains on the surface of the substrate, it still does not solve the problems of bonding strength between abrasive grains and the substrate and utilization rate of cooling medium. For example, the above-mentioned bionic desert beetle self-transport bone micro-grinding head and its preparation process, which is prepared by evenly arranging grooves and arranging abrasive grains in the grooves, cannot ensure the bonding strength of the abrasive grains on the surface of the substrate. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for processing a hydrophilic-hydrophobic composite textured micro-grinding head and a bone micro-grinding device, which can increase the adsorption capacity of the cooling medium and accelerate the condensation speed of fine droplets. At the same time, under the action of abrasive particles and hydrophobic stripes, the droplets can achieve the purpose of rapid self-transportation, reduce the residence time of the droplets on the surface of the coating, and improve the cooling effect of the cooling medium.

[0008] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0009] In a first aspect, an embodiment of the present invention provides a method for processing a hydrophilic-hydrophobic composite texture micro-grinding head, comprising:

[0010] Pre-treating the surface of the micro-grinding head substrate to make the substrate surface rough; and heat-treating the diamond abrasive grains to make them hydrophilic;

[0011] Use a dispensing machine to evenly dispense glue on the surface of the substrate, sprinkle the abrasive particles on the surface of the substrate, and arrange the abrasive particles on the surface of the substrate in an orderly manner;

[0012] The substrate with abrasive particles is placed in a deposition liquid, and a constant voltage DC power supply is used for primary deposition; then, in a deposition liquid with the same composition and the same temperature, the current density is increased for secondary deposition; wherein the secondary deposition time is shorter than the primary deposition time;

[0013] The substrate after the secondary deposition is subjected to acid etching at a set temperature so that the coating on the surface of the substrate forms a hydrophobic surface;

[0014] Laser etching technology is used to form hydrophilic stripes on the hydrophobic surface, so that the hydrophilic stripes and the hydrophobic stripes are distributed alternately.

[0015] As a further implementation method, the deposition liquid includes nickel chloride, boric acid and ethylenediamine hydrochloride in a set ratio, a platinum sheet is connected to the positive electrode, and the substrate is the negative electrode; the temperature of the deposition liquid is 55-65°C, and the current density of the secondary deposition is a multiple of the current density of the initial deposition.

[0016] As a further implementation method, the substrate after the secondary deposition is placed in molten tetradecanoic acid and treated at 75-80° C., then ultrasonically cleaned in a methanol solution at room temperature, and finally taken out and blown dry.

[0017] In a second aspect, an embodiment of the present invention further provides a method for processing a hydrophilic-hydrophobic composite texture micro-grinding head, comprising:

[0018] Pre-treating the surface of the micro-grinding head substrate to make the substrate surface rough; and heat-treating the diamond abrasive grains to make them hydrophilic;

[0019] Wrap a mask with a grid array of holes on a substrate surface coated with photoresist, and cover the mask surface with diamond abrasive grains; vibrate the substrate to distribute the abrasive grains in the array holes of the mask, and after removing the mask, the abrasive grains are arranged in an orderly manner;

[0020] The substrate with abrasive grains is placed in a deposition chamber, the purpose of which is to accelerate the bonding speed between the abrasive grains and the substrate and ensure the bonding strength between the abrasive grains and the substrate. High-purity nitrogen gas carrying heated gaseous nickel is introduced into the deposition chamber, and high-purity hydrogen gas is continuously introduced to deposit the coating under high temperature conditions;

[0021] The photoresist is coated on the surface of the coating and baked at a set temperature; a mask with grid array holes is wrapped on the surface of the substrate, and after ultraviolet exposure, it is placed in a developer and baked again; the substrate after baking and development is acid-etched and fluorinated to obtain a hydrophobic surface;

[0022] Laser etching technology is used to scan the raised parts of the grid to expose the coating at the raised parts; after alkaline etching treatment, a hydrophilic and hydrophobic composite texture micro-grinding head is obtained.

[0023] As a further implementation, the diameter of the holes in the mask is larger than the particle size of a single diamond abrasive grain and smaller than the particle size of two diamond abrasive grains; and the thickness of the mask is 1 / 3 to 2 / 3 of the average particle size of the diamond abrasive grains.

[0024] As a further implementation, the gaseous nickel is heated to 90-100°C, and the substrate temperature of the deposition chamber is maintained at 180-200°C.

[0025] As a further implementation method, the substrate coated with the photoresist is placed on a photoresist-spreading table and rotated at a set speed to obtain a uniformly dispersed photoresist layer; the temperature of the photoresist baking treatment is 90-100°C.

[0026] As a further implementation method, the solution for the acid etching treatment is a mixed acid solution of hydrofluoric acid, nitric acid and water configured in a set mass ratio; and the solution for the fluorination modification is an ethanol solution.

[0027] As a further implementation method, the method for hydrophilizing the abrasive grains is: placing the diamond abrasive grains in a ceramic crucible, loading it into an electric furnace for heat treatment, performing high-temperature heat treatment at a set heating rate, and then annealing and cooling.

[0028] In a third aspect, an embodiment of the present invention further provides a hydrophilic-hydrophobic composite texture bone micro-grinding device, comprising an ultrasonic electric spindle and a micro-grinding head mounted on the ultrasonic electric spindle, wherein the micro-grinding head is manufactured by the processing method described above.

[0029] The beneficial effects of the present invention are as follows:

[0030] (1) The preparation process of the present invention includes substrate surface pretreatment, abrasive grain hydrophilization treatment, orderly arrangement of abrasive grains on the substrate surface, primary deposition, secondary deposition, coating acid etching treatment to form a hydrophobic surface, and laser etching to form hydrophilic stripes, thereby forming a hydrophilic-hydrophobic composite texture micro-grinding head to meet the cooling requirements; and through the primary deposition and secondary deposition, the bonding force between the abrasive grains and the substrate can be increased, and at the same time, by increasing the current density, a pointed cone-shaped micro-nano structure can be formed on the coating surface to improve the hydrophobic performance of the coating; the present invention combines two depositions of electroplated abrasive grains to construct a hydrophilic-hydrophobic composite texture surface, thereby increasing the condensation rate of the cooling medium on the substrate surface and improving the utilization rate of the cooling medium.

[0031] (2) After the abrasive particles are orderly arranged on the surface of the substrate, the present invention can also adopt the steps of deposition to form a coating, baking and developing, fluorination modification, laser etching, and alkaline etching treatment to finally form a hydrophilic and hydrophobic composite texture micro-grinding head structure. After the substrate is alkaline-etched, the original hole structure on the surface of the non-protruding area is reduced, the cracks gradually extend, widen and deepen, and the original protruding structure is deformed to form a new irregular papillary structure. As the alkaline etching time increases, the irregular papillary structure becomes more densely arranged. When the papillary structure is magnified and observed, it can be found that each irregular protrusion is distributed with an interlaced and interconnected mesh-like structure. Due to the presence of the fluorination modification layer, the alkaline etching not only does not damage the previous microstructure, but also forms a new interlaced and interconnected mesh-like hierarchical structure, so that the contact angle and the rolling angle do not change significantly.

[0032] (3) The present invention adopts a method of orderly arranging hydrophilic abrasive particles and combining hydrophilic and hydrophobic composite textures to achieve rapid condensation, transportation, and shedding of the cooling medium. At the same time, it can ensure that the bone chips generated by grinding can be discharged together with the cooling medium, thereby reducing the increase in grinding temperature caused by blockage of the grinding tool. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0034] Figure 1 is a flow chart of Embodiment 1 of the present invention;

[0035] Figure 2 is a flow chart of Embodiment 2 of the present invention;

[0036] Figure 3 is a schematic diagram of abrasive arrangement according to one or more embodiments of the present invention;

[0037] Figure 4 is an enlarged view of the details of the abrasive particle distribution according to one or more embodiments of the present invention;

[0038] Figure 5 is a schematic diagram of the distribution of hydrophilic stripes and hydrophobic stripes according to one or more embodiments of the present invention;

[0039] Figure 6 It is a structural schematic diagram of a bone micro-grinding device according to the third embodiment of the present invention.

[0040] Among them, 1. micro grinding head, 2. ultrasonic electric spindle, 3. diamond abrasive grains, 4. substrate, 5. coating, 6. hydrophilic stripes, 7. hydrophobic stripes. DETAILED DESCRIPTION

[0041] Embodiment 1:

[0042] This embodiment provides a method for processing a hydrophilic-hydrophobic composite texture micro-grinding head. Figure 1 As shown, it includes substrate 4 surface pretreatment, abrasive grain hydrophilization treatment, orderly arrangement of abrasive grains on the substrate 4 surface, primary deposition, secondary deposition, coating 5 acid etching treatment to form a hydrophobic surface, laser etching to form hydrophilic stripes 6, and finally forming a hydrophilic-hydrophobic composite texture micro-grinding head structure.

[0043] The specific production process of the micro-grinding head 1 is as follows:

[0044] Step 1: pre-treat the surface of the substrate 4, that is, degrease, activate and roughen the surface of the substrate 4 before electroplating, in order to increase the bonding force between the coating 5 and the substrate 4 and enhance the corrosion resistance, wear resistance and lubrication functions of the coating 5.

[0045] Since harmful layers such as oxide layers exist on the surface of the substrate 4, the bonding strength between the substrate 4 and the coating 5 is affected. Therefore, it is necessary to use physical or chemical methods to remove harmful substances such as grease and oxides on the surface of the substrate 4, increase the roughness of the surface of the substrate 4, enhance the adhesion between the coating 5 and the substrate 4, and enhance the anti-corrosion and anti-rust performance of the coating 5.

[0046] In this embodiment, the substrate 4 is placed in a degreasing liquid at 80°C, the main components of which include 30 g / L NaOH, 7.5 g / L OP-10 emulsifier, 40 g / L Na2CO3, and 20 g / L Na3PO4, for 20 minutes; then the substrate 4 is activated for 2 minutes using a 10% hydrochloric acid solution, and finally washed and dried with distilled water and anhydrous ethanol in turn. The main purpose is to remove impurities and oxide layers on the surface of the substrate to ensure that nickel can effectively adhere to the surface of the substrate during the electroplating process.

[0047] Step 2: The diamond abrasive grains 3 are hydrophilized to improve the adsorption capacity of the diamond abrasive grains 3 so that the cooling medium droplets can adhere to the abrasive grain surface and enter the grinding area. At the same time, in order to extend the service life of the micro-grinding head 1 and ensure the surface processing quality, diamond abrasive grains 3 with regular shapes and the same size are selected.

[0048] The chemical properties of the abrasive surface determine the speed of condensation of the cooling medium droplets. Diamond abrasive 3 was placed in a ceramic crucible and placed in an electric furnace for heat treatment at 300°C, 400°C, and 500°C at a heating rate of 10°C / min. After completion, it was annealed for 5 hours and then cooled to room temperature.

[0049] Below 300°C, the chemical state of diamond can remain stable, and as the temperature rises, the changes in diamond can be divided into three stages: dehydrogenation, oxidation, and combustion. Therefore, the temperature needs to be controlled to ensure that the diamond does not burn. In the dehydrogenation stage, the hydrogen atoms on the surface of the diamond are desorbed, and as the temperature rises, the surface hydrocarbon groups gradually disappear until they are completely desorbed. In the oxidation stage, oxygen atoms in the air are adsorbed on the surface of the diamond, replacing the hydrogen atoms on the surface on the one hand, and adsorbing on the carbon atoms on the surface on the other hand. Through these two aspects, more oxygen-containing groups carbonyl (C=O) and carboxyl (-COOH) are produced on the surface of the diamond. In the process of increasing oxygen-containing groups, the main increase is the acidic group carboxyl (-COOH), which leads to the formation of carboxylate on the surface of the diamond due to its acidic dissociation. It is under the action of these hydrophilic groups that the diamond surface becomes hydrophilic.

[0050] Step 3: The diamond abrasive grains 3 are arranged in an orderly manner on the surface of the substrate 4.

[0051] The micro-grinding head 1 is fixed on the rotating shaft of the glue dispensing machine. The glue is discharged under the action of the pulse regulator and moves at a uniform speed along the axial direction of the workpiece through the micro-metering head. The micro-grinding head 1 rotates at a certain speed, thereby forming an obliquely ordered glue coating area on the surface of the micro-grinding head 1. Diamond abrasive grains 3 are sprinkled on the substrate 4 to ensure that each glue point can adhere to a diamond abrasive grain 3. The substrate 4 is slightly shaken to make the excess abrasive grains fall off the surface of the substrate 4.

[0052] Step 4: A coating 5 is prepared on the surface of the substrate 4 through primary deposition and secondary deposition. The purpose of the primary deposition is to fix the diamond abrasive grains 3 on the surface of the substrate 4, and the purpose of the secondary deposition is to further increase the bonding force between the abrasive grains and the substrate 4. At the same time, by increasing the current density, a pointed cone-shaped micro-nano structure can be formed on the surface of the coating 5, thereby improving the hydrophobicity of the coating 5.

[0053] During the initial deposition process, as the cathodic polarization process proceeds, the cathodic polarization current density increases sharply. The main reason is that Ni 2+ After gaining electrons, it is reduced to form Ni+ ;Ni + The reduction is continued and nickel is deposited on the surface of the substrate 4. In the secondary deposition process, as the cathode continues to polarize, under the action of ethylenediamine hydrochloride, ethylenediamine hydrochloride nickel ion complex is generated with Ni+ in the electrolyte. The complex is locally discharged on the surface of the substrate 4 during the cathode polarization process to generate nickel and deposit on the surface of the substrate 4.

[0054] Specifically, the substrate 4 is placed in a plating solution with a pH of 4.0 and connected to the negative electrode, and the platinum sheet is connected to the positive electrode. The main components of the plating solution include NiCl2 1mol / L, H3BO3 0.5mol / L, and ethylenediamine hydrochloride 1mol / L. A constant voltage DC power supply is used for electroplating. The current density of the initial deposition is 5A / dm 2 The time is 24min; the current density of the secondary deposition is 10A / dm 2 After the deposition is completed, the substrate 4 is taken out, cleaned and blown dry to obtain a micro-grinding head 1 having a coating 5 that is fine, bright and smooth, with high hardness and wear resistance.

[0055] Due to different current densities during the deposition process, the growth process of the micro-nanostructure on the surface of the substrate 4 is different. When the deposition starts at a lower current density, an obvious micron-scale pointed cone structure gradually grows on the surface of the substrate 4, and as the current density increases, the structure gradually becomes larger, but the height varies; when the current density reaches 5A / dm 2 When the current density reaches 10A / dm 2 , the sizes of the cone-like structures differ again.

[0056] At the same time, as the current density gradually increases, the contact angle will also change significantly, which is mainly related to the change of the surface micro-nano structure. The pointed cone structure generated during the deposition process improves the hydrophobicity of the surface, and as the current density increases, micro-nano secondary structures will be generated locally, further improving the hydrophobicity of the surface.

[0057] Step 5: The coating 5 is subjected to acid etching to form a hydrophobic surface.

[0058] The substrate 4 after the secondary deposition was placed in molten tetradecanoic acid and treated at 80° C. for 60 min. After completion, it was taken out and ultrasonically cleaned in a CH 3 OH solution at room temperature for 2 min, and finally taken out and blown dry.

[0059] Under the action of surface tension, water usually maintains a spherical structure, and the surface of the micro-nano structure is filled with "air chambers". Only when the droplets are small enough can they enter the "air chambers" and fully contact the material, that is, achieve surface wetting. However, in real life, the size of the droplets is larger than the micro-nano-sized "air chambers" and cannot fully contact the material, thus forming surface hydrophobicity.

[0060] The substrate 4 is placed in a molten tetradecanoic acid solution. Since the coating 5 is prone to produce an oxide layer in the air, the oxide layer will react with the tetradecanoic acid. + The shielding of the oxide layer is broken, so that the spontaneous oxidation reaction that originally proceeds slowly on the surface of the coating 5 can be accelerated under acidic conditions and 80° C. until a micro-nano structure is formed on the surface of the coating 5 .

[0061] The nucleation and growth of crystal grains is a process of changing from an ionic state to a solid state, wherein smaller particles dissolve while larger particles continue to grow, thereby increasing the average size of the particles. In the initial stage of immersion, the nickel tetradecanoate content in the solution is low, and as the immersion time increases, Ostwald ripening promotes the growth of cluster crystals on the surface of the coating 5, and smaller polymers grow along the nodules to both sides. As the immersion time of the coating 5 in the tetradecanoic acid solution increases, the nickel tetradecanoate content in the solution increases, and the polymer gradually grows larger, until the nickel tetradecanoate crystals grow around the nodules to form a micro-nano structure, and in addition, the increase in immersion time can make the cluster polymer gradually grow and form on the surface of the coating 5 and tend to be dense, thereby causing a "gas chamber" to be generated between the droplet and the surface of the coating 5, and then forming hydrophobicity to the surface modification.

[0062] The surface of the coating 5 modified with molten myristic acid is covered with a layer of myristic acid. The low surface energy property of the substance further increases the contact angle of the droplet on the coating 5 .

[0063] Step 6: Hydrophobic coating to construct hydrophilic stripes 6.

[0064] Laser etching technology is used to construct the required hydrophilic stripes 6 on the surface of the hydrophobic coating. The laser etching current intensity is 30A, the laser frequency is 30kHz, the number of markings is 1, the marking speed is 1500mm / s, the pulse speed is 10ns, the jump speed is 3000mm / s, the jump delay is 600μm / s, the light-on delay is 500μs, the inflection point delay is 300μs, the light-off delay is 500μs, and the first pulse suppression width is 90μs.

[0065] The hydrophobic mechanism of coating 5 is as follows:

[0066] Generally, the contact angle of the liquid on the surface of the coating 5 is mainly affected by two factors: the roughness of the surface of the coating 5 and the surface energy of the coating 5. Therefore, reducing the surface energy of the coating 5 or increasing the roughness of the surface of the coating 5 can increase the contact angle of the surface of the coating 5, thereby improving the hydrophobic performance.

[0067] According to Wenzel's research on superhydrophobic surfaces, the roughness coefficient can be defined as

[0068]

[0069] Where: S A is the actual rough surface area, S G is the ideal smooth surface area. r is the ratio of the actual solid / liquid interface contact area to the apparent solid / liquid interface contact area, and the relationship is explained according to the following formula:

[0070] cosθ=r cosθ0 (2)

[0071] Where: θ is the contact angle of the rough surface, and θ0 is the contact angle of the ideal smooth surface.

[0072] Assuming that the original surface is an ideal smooth, uniform, and rigid surface, the solid-liquid contact angle is obtained by the Young equation:

[0073]

[0074] Where: γ SV , γ SL , γ LV are the surface tensions of the solid / gas interface, solid / liquid interface, and liquid / gas interface, respectively. The solid-liquid contact angle θ at this time i It is called the intrinsic contact angle of the material. There is a difference between the apparent contact angle of the actual surface and the intrinsic contact angle.

[0075] The so-called surface free energy refers to the surface work that a certain amount of liquid or solid needs to do to increase the surface per unit area at a constant temperature. From the perspective of energy, whether it is liquid or solid, the energy of the surface atoms or molecules is always higher than the energy of the same atoms or molecules inside. The fluidity of the liquid makes the liquid always try to reduce its surface area, thereby reducing the overall energy and making the whole in a more stable state.

[0076] Generally speaking, the surface tensions of solid-gas, liquid-gas, and solid-liquid are different. From a thermodynamic point of view, the following relationship must be satisfied for wetting to occur:

[0077] γ SA ≥γ SL ≥γ LA (4)

[0078] Taking a certain droplet as an example, the volume of the droplet with a radius of R on an ideal solid surface is:

[0079]

[0080] The contact part between the droplet and the air is:

[0081] S=2πR 2 (1-cosθ i ) (6)

[0082] Therefore, the Gibbs free energy of the droplet can be expressed as:

[0083] G=γ LA S-π(R cosθ i ) 2 (γ SA -γ SL ) (7)

[0084] Assuming the volume of the droplet remains constant, then:

[0085]

[0086] By i By taking the derivative, we can verify the Young equation model.

[0087] Wenzel attributed this difference to the fact that the uneven surface of the actual surface caused the increase in the actual contact area between the solid and the liquid, the increase in the solid-liquid and solid-gas interfacial energy, and the liquid completely wetted the grooves on the actual surface, and proposed a full-wetting model; Cassie believed that the difference originated from the difference in surface free energy caused by the uneven surface structure, and pointed out that the contact of the droplet on the rough surface is a composite contact with both solid / liquid and solid / gas contact. He believed that the pits on the rough surface were occupied by trapped gas and the droplet could not enter them, and proposed a full-non-wetting model. The two proposed the apparent contact angle θ and the intrinsic contact angle θ respectively. i Relationship:

[0088] cosθ=r cosθ i (9)

[0089] cosθ=f s (cosθ i +1)-1 (10)

[0090] Where: r is the ratio of the real solid-liquid contact area to the apparent solid-liquid contact area, r>1, f s It is the percentage of solid area on the rough surface.

[0091] Since in actual situations there is both infiltrated liquid and trapped air in the pits on the rough surface, that is, in an intermediate state between the Wenzel state and the Cassie state, a relationship between the two states can be proposed:

[0092]

[0093] Where: a is the diameter of the circular pit, b is the distance between adjacent circles, and x is the infiltration depth.

[0094] In addition to the change in solid-liquid contact area caused by roughness, during the laser microtexturing process, the laser beam irradiates the metal surface, part of which is reflected from the solid surface, and the other part penetrates into its interior and is converted into heat, causing the solid surface energy to increase after processing, thereby increasing the intrinsic contact angle θ of the solid surface. i This is a factor at the material chemical composition level that affects the wettability of the solid surface in addition to the surface microstructure.

[0095] Embodiment 2:

[0096] This embodiment provides a method for processing a hydrophilic-hydrophobic composite texture micro-grinding head. Figure 2 As shown, it includes surface pretreatment of the substrate 4, hydrophilization treatment of the abrasive, orderly arrangement of the abrasive on the surface of the substrate 4, deposition to form a coating 5, baking and developing, fluorination modification, laser etching, and alkaline etching treatment, and finally forming a hydrophilic and hydrophobic composite texture micro-grinding head structure.

[0097] Specifically, the steps include:

[0098] First, the substrate 4 was polished with sandpaper until there were no scratches on the surface, and then ultrasonically cleaned in deionized water, acetone, anhydrous ethanol and distilled water for 10 minutes respectively. After cleaning, it was taken out and blown dry.

[0099] After the substrate 4 is pretreated, a photoresist is coated on its surface, and a mask is laid on the surface of the photoresist. The diameter of the mask hole needs to be larger than the particle size of a single diamond abrasive grain 3 and smaller than the particle size of two diamond abrasive grains 3 to ensure that only one abrasive grain enters the hole, and the thickness of the mask is 1 / 3 to 2 / 3 of the average particle size of the diamond abrasive grain 3.

[0100] Diamond abrasive grains 3 are covered on the surface of the mask, and the substrate 4 is vibrated to make the abrasive grains enter the holes of the mask. After removing the excess diamond abrasive grains 3 outside the holes, the mask is removed and the substrate 4 is placed in the deposition chamber. The purpose is to accelerate the bonding speed between the abrasive grains and the substrate and ensure the bonding strength between the abrasive grains and the substrate; heat the gaseous nickel to 95°C, use 50ml / min high-purity nitrogen to carry the gaseous nickel monomer into the deposition chamber, the substrate 4 temperature of the deposition chamber is maintained at 200°C, the nickel monomer is introduced for 20min, 50ml / min high-purity hydrogen is continuously introduced, and the nickel monomer is repeatedly pulsed. The pressure of the deposition chamber is 3KPa, and a nickel layer of about 20μm is obtained.

[0101] The substrate 4 is coated with photoresist, fixed on a coating table, and rotated at a fixed speed to obtain a flat and evenly dispersed layer of photoresist. After completion, it is placed on a coating table for coating treatment for 10 minutes at a temperature of 100°C. The mask with a grid array of holes is fixed on the surface of the substrate 4, subjected to ultraviolet exposure treatment, and then placed in a developer and gently rotated to ensure uniform development. After the development is completed, the coating is baked again to obtain a layer of yellow film.

[0102] A mixed acid solution is prepared by mixing hydrofluoric acid, nitric acid and water in a mass ratio of 1:2:6, and the treated substrate 4 is placed in the mixed acid solution for acid etching to obtain a grid array structure surface. Finally, acetone, anhydrous ethanol and deionized water are used to clean the substrate 4 in turn to wash away the photoresist film on the surface of the substrate 4, and then the substrate is taken out and dried.

[0103] Furthermore, the substrate 4 was placed in a 1% FAS-17 ethanol solution for fluorination modification for 24 hours. The main substance in the solution is heptadecafluorodecyltrimethoxysilane. In the anhydrous ethanol solution, the Si-O-CH3 group is converted into a Si-OH group. The macromolecule will undergo dehydration condensation with the surface of the substrate 4, and the heptadecafluorodecyltrimethoxysilane molecules will also undergo dehydration condensation reaction, covering the surface of the substrate 4 to form a layer of low surface energy super hydrophobic molecular film, giving the substrate 4 good hydrophobic properties.

[0104] The previously used mask with grid array holes is fixed again on the surface of the substrate 4 to ensure that the mask holes are aligned with the gridded protrusions of the substrate 4. The hydrophobic surface of the grid protrusion surface is scanned through the mask grid holes using laser etching technology, so that the coating 5 is exposed at the protrusion, while the mask shielded part is still in a hydrophobic state.

[0105] Then put the micro-grinding head 1 into a 10 mol / L sodium hydroxide solution and alkaline-etch it at 60°C for 24 hours. After that, wash it with deionized water and dry it in a drying oven at 60°C to enhance the hydrophilic effect of the coating 5 at the protrusions.

[0106] Principle of alkaline etching treatment: After the substrate 4 is alkali-etched, the original hole structure on the surface of the non-protruding area is reduced, the cracks gradually extend, widen and deepen, and the original protruding structure is deformed to form a new irregular papillary structure. As the alkali etching time increases, the irregular papillary structure becomes more densely arranged. When the papillary structure is magnified and observed, it can be found that each irregular protrusion is distributed with an interlaced and interconnected mesh structure. Due to the presence of the fluorinated modification layer, the alkali etching not only does not damage the previous microstructure, but also forms a new interlaced and interconnected mesh hierarchical structure, so that the contact angle and the rolling angle do not change significantly.

[0107] Embodiment three:

[0108] This embodiment provides a hydrophilic-hydrophobic composite texture bone micro-grinding device, such as Figure 6 As shown, it includes an ultrasonic electric spindle 2 and a micro-grinding head 1. The micro-grinding head 1 is mounted on the ultrasonic electric spindle 2, and the micro-grinding head 1 is manufactured by the processing method described in the first or second embodiment.

[0109] like Figure 3-Figure 5 As shown, the micro-grinding head 1 includes a substrate 4, a coating 5 and diamond abrasive grains 3. The diamond abrasive grains 3 are fixed to the surface of the substrate 4 through the coating 5, and the surface of the coating 5 is alternately arranged with hydrophobic stripes 7 and hydrophilic stripes 6 along the circumferential direction. The maximum width of the hydrophilic stripes 6 / hydrophobic stripes 7 is c (100μm~150μm), the thickness of the coating 5 is h (15μm~40μm), and the abrasive grain size is m (48μm~106μm); the abrasive grains are evenly distributed on a circle with a radius of R according to a horizontal interval c and a vertical interval n (20μm~40μm).

[0110] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for processing a hydrophilic and hydrophobic composite texture micro-grinding head, characterized in that: include: Pre-treating the surface of the micro-grinding head substrate to roughen the substrate surface; and heat-treating the diamond abrasive grains to make them hydrophilic; the method for hydrophilizing the abrasive grains is as follows: placing the diamond abrasive grains in a ceramic crucible, loading them into an electric furnace for heat treatment, performing high-temperature heat treatment at a set heating rate, and then annealing and cooling; Wrap a mask with a grid array of holes on a substrate surface coated with photoresist, and cover the mask surface with diamond abrasive grains; vibrate the substrate to distribute the abrasive grains in the array holes of the mask, and after removing the mask, the abrasive grains are arranged in an orderly manner; The substrate with the abrasive particles is placed in a deposition chamber, high-purity nitrogen gas carrying heated gaseous nickel is introduced into the deposition chamber, and high-purity hydrogen gas is continuously introduced to deposit a coating under high temperature conditions; Coating photoresist on the surface of the coating and baking the photoresist at a set temperature; Wrap the mask with grid array holes on the substrate surface, put it into the developer after UV exposure, and bake the glue again; The substrate after the baking and developing process is subjected to acid etching and fluorination modification to obtain a hydrophobic surface; The laser etching technology is used to scan the raised parts of the grid to expose the coating at the raised parts; after alkaline etching treatment, a hydrophilic and hydrophobic composite texture micro-grinding head is obtained; The micro-grinding head was placed in a sodium hydroxide solution and alkali-etched at 60°C. After that, it was washed with deionized water and dried in a drying oven at 60°C.

2. The method for processing a hydrophilic-hydrophobic composite texture micro-grinding head according to claim 1, characterized in that: The hole diameter of the mask is larger than the particle size of a single diamond abrasive grain and smaller than the particle size of two diamond abrasive grains; and the thickness of the mask is 1 / 3 to 2 / 3 of the average particle size of the diamond abrasive grains.

3. The method for processing a hydrophilic-hydrophobic composite texture micro-grinding head according to claim 1, characterized in that: The gaseous nickel is heated to 90~100℃ and the substrate temperature of the deposition chamber is maintained at 180~200℃.

4. The method for processing a hydrophilic-hydrophobic composite texture micro-grinding head according to claim 1, characterized in that: Place the substrate coated with photoresist on a coating table and rotate it at a set speed to obtain a uniformly dispersed coating layer; the temperature of the coating baking treatment is 90~100℃.

5. The method for processing a hydrophilic-hydrophobic composite texture micro-grinding head according to claim 1, characterized in that: The solution for acid etching treatment is a mixed acid solution of hydrofluoric acid, nitric acid and water configured according to a set mass ratio; the solution for fluorination modification is an ethanol solution.

6. A hydrophilic and hydrophobic composite texture bone micro-grinding device, characterized in that: The invention comprises an ultrasonic electric spindle and a micro-grinding head installed on the ultrasonic electric spindle, wherein the micro-grinding head is manufactured by the processing method according to any one of claims 1 to 5.