Calcium-free roasted chromium slag, resource application and preparation method

Through the drying, grinding, screening and ultrasonic washing of calcium-free roasted chromium slag, catalysts for degrading organic pollutants were prepared, and combined with persulfate under visible light, solving the resource utilization of traditional chromite treatment methods. The problems of insufficient utilization and difficulty in degrading organic pollutants have been achieved, efficient pollutant degradation and high-value utilization of chromium slag resources.

CN117263357BActive Publication Date: 2024-11-15CHONGQING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311202491.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-18
Publication Date
2024-11-15
Estimated Expiration
2043-09-18

AI Technical Summary

Technical Problem

Traditional chromite treatment methods have problems such as insufficient resource utilization, difficult recycling and high cost, and it is difficult to effectively degrade organic pollutants in the water environment.

Method used

Calcium-free calcined chromium slag is used as a catalyst, and the water-washed chromium slag catalyst is prepared by drying, grinding, screening and ultrasonic washing, and combined with persulfate under visible light to activate the generation of free radicals to degrade organic pollutants.

Benefits of technology

It significantly improves the degradation effect of organic pollutants, realizes the resource utilization of calcium-free roasted chromium slag, reduces the threat of chromium slag to the ecological environment, and replaces commercial catalysts, with stable performance, high catalytic activity, easy to recover and repeat Advantages of good sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117263357B_ABST
    Figure CN117263357B_ABST
Patent Text Reader

Abstract

The present invention relates to a calcium-free roasted chromium slag, resource application and preparation method. Resource application of calcium-free roasted chromium slag, application of the calcium-free roasted chromium slag in degrading organic pollutants. The present invention also provides a preparation method of the calcium-free roasted chromium slag for resource application as described in the present invention, comprising the following steps: drying, grinding and screening the calcium-free roasted chromium slag to obtain a chromium slag raw material; adding water to the chromium slag raw material, ultrasonically treating, filtering, and drying to obtain a water-washed chromium slag catalyst, wherein the water-washed chromium slag catalyst is the calcium-free roasted chromium slag for resource application. The present invention also provides a calcium-free roasted chromium slag for resource application as described in the present invention, which is prepared by the preparation method described in the present invention. The present invention effectively realizes the resource utilization of calcium-free roasted chromium slag, alleviates the problem of secondary potential resource waste caused by chromium slag, and reduces the threat of chromium slag to the ecological environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to calcium-free roasted chromium slag, resource application and preparation method thereof. Background Art

[0002] Due to the rapid development of industry and agriculture, various organic pollutants are frequently detected in the water environment. These pollutants not only induce biological resistance and cause endocrine disorders in the human body, but also pose a serious threat to the ecological environment. At present, it is difficult to effectively remove organic pollutants by traditional sewage treatment methods. The advanced oxidation process (AOP) based on peroxymonosulfate (PMS) activation has good application prospects in the degradation of antibiotics (tetracycline, ciprofloxacin, levofloxacin, etc.). This is because PMS is easily activated to produce strong oxidative free radicals (SO4•- and •OH) that can convert large-molecule antibiotics into harmless small molecules, thereby reducing water pollution. However, synthetic catalysts usually have problems such as complex preparation, expensive material costs, and low synthesis efficiency. Therefore, it is crucial to find catalysts that are inexpensive, simple to manufacture, responsive to visible light, and have highly active redox surfaces.

[0003] Calcium-free roasted chromium slag (COPR) is a solid waste produced after deep extraction of chromium from chromite at high temperature (1100~1200 °C). Traditional treatment methods for chromium slag include acid leaching, alkaline leaching, carbon thermal reduction, etc. The acid leaching method for chromium slag has an ideal metal leaching effect and a simple method, but due to the high cost, strong acidity and poor selectivity of the acid, the recovery of metal elements through indiscriminate leaching greatly increases the difficulty of subsequent separation; although the alkaline leaching method for chromium slag can achieve selective leaching of Cr, it will have problems such as high alkali consumption, difficult alkali recovery, and difficult separation of chromium and alkali; although carbon thermal reduction achieves selective recovery of metals, the reduction temperature is high, the energy consumption is large, and the recovered metal grade is low. Therefore, the above methods of chromite resource utilization generally have a series of problems such as insufficient resource utilization, difficulty in recovery, complex operation, and high cost. Summary of the invention

[0004] The purpose of the present invention is to provide a calcium-free roasted chromium slag, resource application and preparation method, so as to effectively realize the resource utilization of the calcium-free roasted chromium slag, alleviate the problem of secondary potential resource waste caused by chromium slag, and reduce the threat of chromium slag to the ecological environment.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A resource application of calcium-free roasted chromium slag, and application of the calcium-free roasted chromium slag in degrading organic pollutants.

[0007] According to the above-mentioned technical means, experiments have proved that the use of calcium-free roasted chromium slag in the degradation of organic pollutants can significantly improve the degradation effect of organic pollutants, thereby effectively realizing the resource utilization of calcium-free roasted chromium slag, and then effectively alleviating the problem of secondary potential resource waste caused by chromium slag, and reducing the threat of chromium slag to the ecological environment.

[0008] The calcium-free roasted chromium slag of the present invention can replace commercial catalysts such as Al2O3, SiO2, MgO, Fe2O3, etc., not only effectively realizes the restoration of environmental pollution, but also realizes the high-value resource application of chromium slag solid waste. The solid waste calcium-free roasted chromium slag is applied to the restoration of environmental problems, effectively realizing the environmental goal of "treating waste with waste". Experiments have proved that the calcium-free roasted chromium slag of the present invention has stable performance, high catalytic activity, and is suitable for a variety of antibiotic wastewater and dye wastewater, and the catalyst has the advantages of magnetism, easy recovery, and good repeatability.

[0009] Preferably, the calcium-free calcined chromium slag is used as a catalyst in degrading organic pollutants in sewage.

[0010] Preferably, the calcium-free roasted chromium slag is used as an activator of persulfate in degrading organic pollutants in sewage.

[0011] Preferably, the calcium-free calcined chromium slag is used as an activator of persulfate in the degradation of organic pollutants in sewage with the assistance of visible light.

[0012] Experiments have proved that, with the assistance of visible light, when calcium-free roasted chromium slag and persulfate are added to wastewater containing organic pollutants, the iron oxide, magnesium ferrite and unreacted chromite components in the calcium-roasted chromium slag can activate persulfate to produce hydroxyl radicals, sulfate radicals, superoxide radicals and singlet oxygen, thereby effectively achieving the degradation of organic matter; at the same time, the natural combination of mineral phases such as magnesium ferrite, ferrous oxide and chromite in the calcium-free roasted chromium slag makes the chromium slag itself have a narrow band gap, which makes it easy to achieve the separation of electrons and holes under visible light, which is conducive to achieving visible light response and further promoting the continued degradation reaction.

[0013] Preferably, the concentration of persulfate in the sewage is 3-5 mM, the stirring rate after adding calcium-free calcined chromium slag and persulfate to the sewage is 100-200 rpm, and the degradation reaction time is 60 min.

[0014] Preferably, the organic pollutant includes at least one of tetracycline (TC), methyl orange (MO) and levofloxacin (LEV).

[0015] Preferably, the concentration of the calcium-free roasted chromium slag in degrading organic pollutants in sewage is 0.5-1 g / L.

[0016] Preferably, the concentration of organic pollutants in the sewage is 20-40 mg / L.

[0017] The present invention also provides a method for preparing the calcium-free roasted chromium slag for resource utilization as described in the present invention, comprising the following steps:

[0018] S1, drying, grinding and screening the calcium-free roasted chromium slag to obtain a chromium slag raw material;

[0019] S2. Add water to the chromium slag raw material, mix and treat, filter, take out the chromium slag, repeatedly add water, ultrasonically treat and filter for more than three times to fully remove the mobile hexavalent chromium, dry and obtain a water-washed chromium slag catalyst, which is a calcium-free roasted chromium slag for resource application.

[0020] According to the above technical means, by drying, grinding, screening and ultrasonic water washing the calcium-free calcined chromium slag, a washed chromium slag catalyst for degrading organic pollutants in wastewater can be obtained. This catalyst has the advantages of simple process, cleanliness and excellent photocatalytic performance, thereby effectively realizing the high value-added resource application of calcium-free calcined chromium slag.

[0021] Among them, the hexavalent chromium content in the filtrate after filtration is far lower than the requirements of the national standard for general industrial solid waste.

[0022] Preferably, in S1, the calcium-free roasted chromium slag is solid waste generated by a calcium-free roasting process of chromite ore to prepare chromium salt products.

[0023] Preferably, in S1, the particle size of the chromium slag raw material obtained after screening is less than 0.075 mm (greater than 200 mesh).

[0024] By controlling the particle size of the chromium slag raw material obtained after screening treatment to be less than 0.075 mm, it is beneficial to increase the specific surface area of ​​the water-washed chromium slag catalyst and to carry out the efficient activation application of the water-washed chromium slag catalyst.

[0025] Preferably, in S2, the mixing treatment includes at least one of ultrasonic treatment, shaking treatment and centrifugal treatment.

[0026] Preferably, the frequency of ultrasonic treatment is 20-40 KHz, and the power is 300-600 W.

[0027] Preferably, the frequency of ultrasonic treatment is 40KHz and the power is 600W.

[0028] Preferably, the shaking table treatment has a rotation speed of 200-350 r / min and a treatment time of 1-3 h.

[0029] Preferably, the rotation speed of the centrifugal treatment is 4000-6000 r / min, and the time is 5-15 min.

[0030] Preferably, the centrifugal treatment speed is 5000r / min and the time is 10min.

[0031] Preferably, the water in S2 is deionized water.

[0032] By controlling the frequency and power of ultrasonic treatment, the transfer of mobile hexavalent chromium in the chromium slag to water is effectively guaranteed.

[0033] Preferably, filtration is performed using a 0.22-0.45 μm mixed cellulose filter membrane.

[0034] Preferably, filtration is performed using a 0.45 μm mixed cellulose filter membrane.

[0035] Filtration with a 0.45 μm mixed cellulose membrane is beneficial for liquid-solid separation of chromium slag and aqueous solution containing hexavalent chromium.

[0036] Preferably, in S2, the liquid-to-solid ratio of water to the chromium slag raw material is 100:1 to 20:1.

[0037] By controlling the liquid-solid ratio of water to chromium slag raw materials between 100:1 and 20:1, the chromium slag is effectively guaranteed to be in full contact with deionized water, thereby fully transferring the mobile hexavalent chromium into the deionized water.

[0038] Preferably, the drying temperature is 60°C to 120°C, and the drying time is 12 to 24 hours.

[0039] Preferably, the drying time is 24 hours.

[0040] The present invention also provides a calcium-free roasted chromium slag for resource utilization as described in the present invention, which is prepared by the preparation method described in the present invention.

[0041] Beneficial effects of the present invention:

[0042] 1) The resource application of the calcium-free roasted chromium slag of the present invention, using the calcium-free roasted chromium slag in the degradation of organic pollutants can significantly improve the degradation effect of organic pollutants, thereby effectively realizing the resource utilization of the calcium-free roasted chromium slag, and then effectively alleviating the problem of secondary potential resource waste caused by chromium slag, and reducing the threat of chromium slag to the ecological environment; the calcium-free roasted chromium slag of the present invention can replace commercial catalysts such as Al2O3, SiO2, MgO, Fe2O3, etc., not only effectively realizing the restoration of environmental pollution, but also realizing the high-value resource application of chromium slag solid waste, and applying the solid waste calcium-free roasted chromium slag to the restoration of environmental problems, effectively realizing the environmental goal of "waste treatment with waste", and the experiment proves that the calcium-free roasted chromium slag of the present invention has the advantages of stable performance, high catalytic activity, and is applicable to a variety of antibiotic wastewater and dye wastewater, and the catalyst has the advantages of magnetism, easy recovery, and good repeatability;

[0043] 2) The method for preparing calcium-free roasted chromium slag of the present invention can obtain a washed chromium slag catalyst for degrading organic pollutants in sewage by drying, grinding, screening and ultrasonic water washing the calcium-free roasted chromium slag. The method has the advantages of simple process, cleanliness and excellent photocatalytic performance, thereby effectively realizing the high value-added resource application of calcium-free roasted chromium slag, and has promotion and application value in the field of chromium slag resource utilization and catalyst technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is a flow chart of the method for preparing calcium-free roasted chromium slag of the present invention;

[0045] Figure 2 This is a SEM morphology image of the water-washed chromium slag catalyst prepared in Example 1 at 500 times magnification;

[0046] Figure 3 This is a SEM morphology image of the water-washed chromium slag catalyst prepared in Example 1 at a magnification of 10,000 times;

[0047] Figure 4 This is a SEM morphology image of the water-washed chromium slag catalyst prepared in Example 1 at a magnification of 20,000 times;

[0048] Figure 5 This is a diagram showing the degradation effect of the organic pollutant tetracycline (TC) degraded by the water-washed chromium slag catalyst;

[0049] Figure 6 This is a diagram showing the degradation effect of the organic pollutant methyl orange (MO) by the water-washed chromium slag catalyst;

[0050] Figure 7 This is a diagram showing the degradation effect of the organic pollutant levofloxacin (LEV) by the water-washed chromium slag catalyst;

[0051] Figure 8This is a diagram showing the cyclic degradation effect of water-washed chromium slag catalyst. DETAILED DESCRIPTION

[0052] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0053] Example 1

[0054] like Figure 1 As shown, a method for preparing calcium-free roasted chromium slag comprises the following steps:

[0055] S1. Place the calcium-free calcined chromium slag in a blast drying oven at 80°C for 24 hours, then use a ball mill to mill for 2 hours and then sieve to obtain a chromium slag raw material with a particle size of less than 0.075 mm (greater than 200 mesh);

[0056] S2, adding deionized water to the chromium slag raw material at a liquid-to-solid ratio of 100:1 to obtain a mixed solution, and subjecting the mixed solution to ultrasonic treatment for 10 minutes using 600W, 40KHz ultrasound;

[0057] S3, use a vacuum filtration pump to filter the mixed solution under a 0.45 μm mixed cellulose filter membrane, remove the filter residue and repeat S2 three or more times to fully remove the migratable hexavalent chromium;

[0058] S4. The filtered chromium slag is subjected to low-temperature drying treatment in a 60°C forced air drying oven for 24 h to obtain a water-washed chromium slag catalyst.

[0059] Example 2

[0060] A method for preparing calcium-free roasted chromium slag comprises the following steps:

[0061] S1. Place the calcium-free calcined chromium slag in a blast drying oven at 80°C for 24 hours, then use a ball mill to mill for 2 hours and then sieve to obtain a chromium slag raw material with a particle size of less than 0.075 mm (greater than 200 mesh);

[0062] S2. Add deionized water to the chromium slag raw material at a liquid-to-solid ratio of 100:1 to obtain a mixed solution, and use a shaker to shake the solution at 200-350 r / min for 2 h at room temperature;

[0063] S3, use a vacuum filtration pump to filter the mixed solution under a 0.45 μm mixed cellulose filter membrane, remove the filter residue and repeat S2 three or more times to fully remove the migratable hexavalent chromium;

[0064] S4. The filtered chromium slag is subjected to low-temperature drying treatment in a 60°C forced air drying oven for 24 h to obtain a water-washed chromium slag catalyst.

[0065] Example 3

[0066] A method for preparing calcium-free roasted chromium slag comprises the following steps:

[0067] S1. Place the calcium-free calcined chromium slag in a blast drying oven at 80°C for 24 hours, then use a ball mill to mill for 2 hours and then sieve to obtain a chromium slag raw material with a particle size of less than 0.075 mm (greater than 200 mesh);

[0068] S2, adding deionized water to the chromium slag raw material at a liquid-to-solid ratio of 10:1 to obtain a mixed solution, and centrifuging the solution at 5000 r / min for 10 min at room temperature using a centrifuge;

[0069] S3, use a vacuum filtration pump to filter the mixed solution under a 0.45 μm mixed cellulose filter membrane, remove the filter residue and repeat S2 three or more times to fully remove the migratable hexavalent chromium;

[0070] S4. The filtered chromium slag is subjected to low-temperature drying treatment in a 60°C forced air drying oven for 24 h to obtain a water-washed chromium slag catalyst.

[0071] Example 4

[0072] A method for resource utilization of calcium-free roasted chromium slag is to activate persulfate (potassium peroxymonosulfate salt - PMS, molecular formula K2O5S) under visible light with the washed chromium slag catalyst prepared in Example 1, and degrade tetracycline (TC), an organic pollutant in water, and the specific steps are as follows:

[0073] The washed chromium slag catalyst and persulfate (PMS) prepared in Example 1 were added to sewage containing the organic pollutant tetracycline (TC) and mixed evenly, wherein the concentration of tetracycline (TC) in the sewage was 20 mg / L, the volume of the sewage was 100 mL, the amount of the washed chromium slag catalyst added was 0.5 g / L, the concentration of persulfate (PMS) was 3 mM, and the power of visible light was 45 W; magnetic stirring was performed at room temperature for 60 min.

[0074] Example 5

[0075] A method for resource utilization of calcium-free roasted chromium slag is to activate persulfate (potassium peroxymonosulfate salt - PMS, molecular formula K2O5S) under visible light with the washed chromium slag catalyst prepared in Example 1, and degrade methyl orange (MO), an organic pollutant in water, and the specific steps are as follows:

[0076] The washed chromium slag catalyst and persulfate (PMS) prepared in Example 1 were added to sewage containing the organic pollutant methyl orange (MO) and mixed evenly, wherein the concentration of methyl orange (MO) in the sewage was 20 mg / L, the volume of the sewage was 100 mL, the addition amount of the washed chromium slag catalyst was 0.5 g / L, the concentration of persulfate (PMS) was 3 mM, and the power of visible light was 45 W; magnetic stirring was performed at room temperature for 60 min.

[0077] Example 6

[0078] A method for resource utilization of calcium-free roasted chromium slag is to activate persulfate (potassium peroxymonosulfate salt - PMS, molecular formula K2O5S) under visible light with the washed chromium slag catalyst prepared in Example 1, and degrade the organic pollutant levofloxacin (LEV) in the water body, and the specific steps are as follows:

[0079] The washed chromium slag catalyst and persulfate (PMS) prepared in Example 1 were added to sewage containing the organic pollutant levofloxacin (LEV) and mixed evenly, wherein the concentration of levofloxacin (LEV) in the sewage was 20 mg / L, the volume of the sewage was 100 mL, the amount of the washed chromium slag catalyst added was 0.5 g / L, the concentration of persulfate (PMS) was 3 mM, and the power of visible light was 45 W; magnetic stirring was performed at room temperature for 60 min.

[0080] Detection and analysis

[0081] 1) The washed chromium slag catalyst prepared in Example 1 was subjected to scanning electron microscopy analysis, and the results were as follows: Figures 2 to 4 shown.

[0082] Figure 2 This is the SEM morphology of the water-washed chromium slag catalyst at 500 times magnification. Figure 3 This is the SEM morphology of the water-washed chromium slag catalyst at 10,000 times magnification. Figure 4 This is a SEM morphology of the water-washed chromium slag catalyst at 20,000 times magnification. Figures 2 to 4 From the analysis, it can be seen that the water-washed chromium slag catalyst has regular crystal shape, compact texture, smooth surface, and is not easy to be damaged. It can prevent the leaching of metal ions and reduce the loss of catalytic structure to a large extent.

[0083] 2) The absorbance of the solution in the reaction system of Examples 4 to 6 was measured in a UV-visible spectrophotometer system, wherein the absorbance of the organic pollutant tetracycline (TC) was measured at 357 nm, the absorbance of the organic pollutant methyl orange (MO) was measured at 463 nm, and the absorbance of the organic pollutant levofloxacin (LEV) was measured at 288 nm. When the organic pollutant tetracycline (TC) was measured, the addition of washed chromium slag catalyst (COPR), only persulfate (PMS), only under visible light, under washed chromium slag catalyst (COPR) + visible light, and washed chromium slag catalyst (COPR) + persulfate (PMS) were used as controls. The results are as follows: Figures 5 to 7 shown.

[0084] Figure 5 This is the degradation effect diagram of the organic pollutant tetracycline (TC) degraded by the water-washed chromium slag catalyst. Figure 5 It can be seen from the analysis that after 60 minutes of reaction, the degradation rate of the organic pollutant tetracycline (TC) can reach 94.37%, which proves that the washed chromium slag catalyst prepared in Example 1 has an excellent degradation effect on tetracycline (TC).

[0085] Figure 6 This is the degradation effect diagram of the organic pollutant methyl orange (MO) degraded by the water-washed chromium slag catalyst. Figure 6 It can be seen from the analysis that after 60 minutes of reaction, the degradation rate of the organic pollutant methyl orange (MO) can reach 96.24%, which proves that the washed chromium slag catalyst prepared in Example 1 has an excellent degradation effect on methyl orange (MO).

[0086] Figure 7 This is the degradation effect diagram of the organic pollutant levofloxacin (LEV) degraded by the washed chromium slag catalyst. Figure 7 It can be seen from the analysis that after 60 minutes of reaction, the degradation rate of the organic pollutant levofloxacin (LEV) can reach 87.02%, which proves that the washed chromium slag catalyst prepared in Example 1 has an excellent degradation effect on levofloxacin (LEV).

[0087] 3) Cyclic degradation test

[0088] The washed chromium slag catalyst prepared in Example 1 was activated with persulfate (potassium peroxymonosulfate salt - PMS) under visible light, and the organic pollutant tetracycline (TC) in the water was degraded for 5 cycles. The specific steps are as follows:

[0089] The washed chromium slag catalyst and persulfate (PMS) prepared in Example 1 were added to the sewage containing the organic pollutant tetracycline (TC) and mixed evenly, wherein the concentration of tetracycline (TC) in the sewage was 20 mg / L, the sewage volume was 100 mL, the amount of the washed chromium slag catalyst added was 0.5 g / L, the concentration of persulfate (PMS) was 3 Mm, and the power of visible light was 45 W; magnetic stirring was performed at room temperature for 60 min. After the degradation was completed, the mixed solution was filtered under a 0.45 μm mixed cellulose filter membrane using a vacuum filtration pump, the filter residue was removed and the above degradation steps were repeated four times to complete the cyclic degradation experiment. The results are as follows Figure 8 shown.

[0090] from Figure 8 From the analysis, it can be seen that the degradation results of the five cycles are 94.37%, 91.54%, 87.55%, 86.01% and 85.07% respectively, which proves that the washed chromium slag catalyst prepared in Example 1 has a stable material structure and excellent cycle characteristics.

[0091] In summary, the resource application of the calcium-free roasted chromium slag of the present invention, using the calcium-free roasted chromium slag for the degradation of organic pollutants, can significantly improve the degradation effect of organic pollutants, thereby effectively realizing the resource utilization of the calcium-free roasted chromium slag, and then effectively alleviating the problem of secondary potential resource waste caused by chromium slag, and reducing the threat of chromium slag to the ecological environment; the calcium-free roasted chromium slag of the present invention can replace commercial catalysts such as Al2O3, SiO2, MgO, Fe2O3, etc., not only effectively realizing the remediation of environmental pollution, but also realizing the high-value resource application of chromium slag solid waste, and applying the solid waste calcium-free roasted chromium slag to the remediation of environmental problems, effectively realizing the environmental goal of "treating waste with waste", and experiments have proved that the calcium-free roasted chromium slag of the present invention has stable performance, high catalytic activity, is applicable to a variety of antibiotic wastewater and dye wastewater, and the catalyst has the advantages of magnetism, easy recovery and good repeatability.

[0092] The method for preparing calcium-free roasted chromium slag of the present invention can obtain a washed chromium slag catalyst for degrading organic pollutants in sewage by drying, grinding, screening and ultrasonic water washing the calcium-free roasted chromium slag. The method has the advantages of simple process, cleanliness and excellent photocatalytic performance, thereby effectively realizing the high-value-added resource application of the calcium-free roasted chromium slag, and has promotion and application value in the field of chromium slag resource utilization and catalyst technology.

[0093] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A resource application of calcium-free roasted chromium slag, characterized in that: The calcium-free roasted chromium slag is used as an activator of potassium peroxymonosulfate salt in the degradation of organic pollutants in sewage under the assistance of visible light; The method for preparing the calcium-free roasted chromium slag comprises the following steps: S1, drying, grinding and screening the calcium-free roasted chromium slag to obtain a chromium slag raw material; S2. Add water to the chromium slag raw material, mix and treat, filter to fully remove the mobile hexavalent chromium, dry and obtain a water-washed chromium slag catalyst, wherein the water-washed chromium slag catalyst is a calcium-free roasted chromium slag for resource utilization.

2. The resource utilization of calcium-free roasted chromium slag according to claim 1, characterized in that: The organic pollutant includes at least one of tetracycline (TC), methyl orange (MO) and levofloxacin (LEV).

3. The resource utilization of calcium-free roasted chromium slag according to claim 1, characterized in that: The calcium-free roasted chromium slag is used to degrade organic pollutants in sewage, and the concentration of the calcium-free roasted chromium slag is 0.5-1 g / L.

4. The resource utilization of calcium-free roasted chromium slag according to claim 1, characterized in that: In S2, the mixing treatment includes at least one of ultrasonic treatment, shaking treatment and centrifugal treatment; The frequency of ultrasonic treatment is 20~40kHz, and the power is 300~600W; The speed of the shaking table treatment is 200~350r / min, and the time is 1~3h; The speed of centrifugal treatment is 4000~6000r / min, and the time is 5~15min; And / or, filtering is performed using a 0.22-0.45 μm mixed cellulose filter membrane.

5. The resource utilization of calcium-free roasted chromium slag according to claim 1, characterized in that: In S2, the liquid-to-solid ratio of water to the chromium slag raw material is 100:1-20:1; And / or, the drying temperature is 60°C to 120°C, and the drying time is 12 to 24 hours.