A ceramic and its preparation method and application
By adding BaAl12O19 and 3Al2O3·2SiO2 to ceramic materials, combined with yttria-stabilized zirconia, the problems of high density and insufficient impact resistance of ceramic materials are solved, and low density, high impact resistance and low sintering temperature of ceramic materials are achieved. Suitable for electronic product casings, promoting industrial production and energy saving.
Patent Information
- Application Number
- CN202210729176.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-06-24
AI Technical Summary
Existing ceramic materials have high density and insufficient impact resistance. The high sintering temperature is not conducive to industrial production. It is difficult to balance the requirements of material density, impact resistance and low sintering temperature.
Ceramic materials containing BaAl12O19, 3Al2O3·2SiO2 and yttria-stabilized zirconia are used to prepare ceramic powder through a wet grinding method and sintered at a lower temperature to form a ceramic with high impact resistance and low dielectric constant.
The ceramic material has lower density, higher impact resistance, lower sintering temperature, is suitable for electronic product housing applications, and promotes industrial production and energy saving.
Smart Images

Figure BDA0003712234960000161
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramics, and in particular to ceramics and a preparation method and application thereof. Background Art
[0002] When existing ceramics such as yttria-stabilized zirconia ceramics are used in electronic product housings, they have a high density, resulting in a heavier product, and their dielectric constant is high, which will affect the stable transmission of electronic product signals to a certain extent. A prior art discloses adding alumina to zirconia ceramics to reduce the density and dielectric constant of the resulting ceramic material, but the impact resistance of the ceramic is reduced. If it is necessary to obtain ceramics that meet the density requirements of industrial products, the sintering temperature needs to reach 1600 degrees or even higher. Therefore, it becomes important to develop ceramics with relatively low material density, high impact resistance, and low sintering temperature. Summary of the invention
[0003] The purpose of the present invention is to overcome the problems of relatively low material density, high impact resistance and low sintering temperature of existing ceramics, and to provide a ceramic and a preparation method and application thereof.
[0004] In order to achieve the above object, the present invention provides a ceramic in the first aspect, wherein the ceramic phase contains: 30-70wt% BaAl 12 O 19 , 0.5-4.66wt% of 3Al2O3·2SiO2 (i.e. mullite), and 25.34-69.5wt% of yttria-stabilized zirconia.
[0005] Preferably, the ceramic phase contains: 40-60 wt% BaAl 12 O 19 , 0.67-4wt% 3Al2O3·2SiO2, 36-59.33wt% yttria-stabilized zirconia.
[0006] Optionally, the molar ratio of yttria to zirconia contained in the yttria-stabilized zirconia is (1.5-4):(98.5-96).
[0007] Preferably, in the drop weight impact test results of the ceramic, the average drop weight height is greater than or equal to 25 cm.
[0008] Preferably, in the density test results of the ceramic, the average number of pits with a pit diameter greater than 20 μm within a range of 10×10 mm is 0.
[0009] Optionally, the sintering temperature required to prepare the above ceramic is equal to or less than 1500 degrees Celsius.
[0010] A second aspect of the present invention provides a method for preparing a ceramic, comprising:
[0011] (1) adding water, a dispersant and a binder to a powder containing barium oxide, aluminum oxide, yttria-stabilized zirconium oxide and 3Al2O3·2SiO2 (i.e., mullite) and performing wet grinding to obtain a slurry;
[0012] (2) drying the slurry to obtain ceramic powder;
[0013] (3) The ceramic powder is molded and then sintered in air to obtain ceramics.
[0014] In the powder, the content of barium oxide is 6.01-14.02wt%, the content of aluminum oxide is 23.98-55.95wt%, the content of yttria-stabilized zirconium oxide is 25.34-69.5wt%, and the content of 3Al2O3·2SiO2 is 0.5-4.66wt%;
[0015] Preferably, the content of barium oxide is 8.01-12.02wt%, the content of aluminum oxide is 31.97-47.96wt%, the content of yttria-stabilized zirconia is 36-59.33wt%, and the content of 3Al2O3·2SiO2 is 0.67-4wt%.
[0016] Optionally, the molar ratio of yttria to zirconium oxide contained in the yttria-stabilized zirconia is (1.5-4): (98.5-96)
[0017] Optionally, the molding may be performed by one of dry pressing, isostatic pressing, injection molding, and hot die casting.
[0018] Optionally, the dispersant is selected from at least one of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose and triethanolamine; the binder is selected from polyvinyl alcohol and / or polyethylene glycol 4000;
[0019] Optionally, the dispersant is added in an amount of 0.005-0.5% by weight of the powder, preferably 0.01-0.1% by weight;
[0020] Optionally, the amount of the binder added is 0.5-5% by weight of the powder, preferably 2-5% by weight;
[0021] Preferably, the solid content of the slurry is 20-60 wt %, preferably 25-55 wt %.
[0022] Preferably, the sintering procedure includes: heating from room temperature to 600°C over 400 minutes and keeping warm for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping warm for 2 hours, heating from 1150°C to 1400-1500°C over 150 minutes and keeping warm for 1-2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0023] The third aspect of the present invention provides a ceramic produced by the preparation method of the present invention.
[0024] A fourth aspect of the present invention provides an application of the ceramic provided by the present invention in preparing an electronic product housing.
[0025] The ceramic of the present invention introduces BaAl 12 O 19 , so that the obtained ceramic material has a lower density. Although the alumina-modified zirconia ceramics in the prior art have a lower density, their impact resistance is lower, while the impact resistance of the ceramics of the present invention is very good. The inventors of the present invention analyzed that BaAl 12 O 19 At high temperatures, the grains grow longer to form whiskers, thereby enhancing the impact resistance of the ceramic of the present invention. Moreover, the ceramic of the present invention has a lower dielectric constant than the existing yttria-stabilized zirconia ceramics, which is beneficial for its application in stable signal transmission in electronic products. The introduction of 3Al2O3·2SiO2 (i.e., mullite) into the ceramic material of the present invention can greatly reduce the sintering temperature and, to a certain extent, is beneficial for further improving the impact resistance, so that the sintering temperature required for the ceramic with qualified density (i.e., in the density test results of the ceramic, the average number of pits with a pit diameter greater than 20μm within every 10×10mm is 0) is equal to or less than 1500 degrees. The low sintering temperature does not require a high sintering furnace, which is beneficial for large-scale industrial production, and the low sintering temperature is beneficial for energy saving and green production. DETAILED DESCRIPTION
[0026] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0027] The first aspect of the present invention provides a ceramic, wherein the ceramic phase contains: 30-70wt% BaAl 12 O 19 , 0.5-4.66wt% of 3Al2O3·2SiO2, and 35.34-69.5wt% of yttria-stabilized zirconia.
[0028] The ceramic of the present invention introduces BaAl 12 O 19 , so that the obtained ceramic material has a lower density. Although the alumina-modified zirconia ceramics in the prior art have a lower density, their impact resistance is lower, while the impact resistance of the ceramics of the present invention is very good. The inventors of the present invention analyzed that BaAl 12 O 19 At the sintering temperature, the grains grow longer to form whiskers, thereby enhancing the impact resistance of the ceramic of the present invention. Moreover, the ceramic of the present invention has a lower dielectric constant than the existing pure yttria-stabilized zirconia ceramics, which is beneficial to its application in stable signal transmission in electronic products. The introduction of 3Al2O3·2SiO2 (i.e., mullite) into the ceramic material of the present invention can greatly reduce the sintering temperature and, to a certain extent, is beneficial to further improve the impact resistance, so that the sintering temperature required for the ceramic with qualified density (i.e., in the density test results of the ceramic, the average number of pits with a pit diameter greater than 20μm within every 10×10mm is 0) is equal to or less than 1500 degrees. The low sintering temperature does not require a high sintering furnace, which is beneficial to large-scale industrial production, and the low sintering temperature is beneficial to energy saving and green production.
[0029] The inventors of the present invention have found through a large number of experiments that BaAl 12 O 19 The content of BaAl is 30-70wt%, because too low a content is not conducive to reducing the density of ceramic products, and BaAl 12 O 19 Too high a content will lead to a decrease in the impact resistance of the product, that is, a decrease in the average drop height. The 3Al2O3·2SiO2 content is 0.5-4.66wt%. A too low 3Al2O3·2SiO2 content is not conducive to reducing the sintering temperature in the preparation process of ceramic products, is not conducive to large-scale industrial production, and is not conducive to energy conservation; a too high 3Al2O3·2SiO2 content will lead to a decrease in the impact resistance of the product, that is, a decrease in the average drop height. The yttria-stabilized zirconia content is 35.34-69.5wt%. A too low yttria-stabilized zirconia content will cause the ceramic to crack during sintering; and a too high yttria-stabilized zirconia content will result in a higher dielectric constant of the ceramic product, which is not conducive to the stable transmission of electrical signals when it is used in electronic products. Therefore, based on the above analysis, each component in the ceramic product of the present invention is important in the ceramic product, and they together constitute the ceramic of the present invention.
[0030] Preferably, the ceramic phase contains: 40-60wt% BaAl 12 O 19, 0.67-4wt% 3Al2O3·2SiO2, 36-59.33wt% yttria-stabilized zirconia. The inventors of the present invention have found through a large number of experiments that in the drop hammer impact test results of the ceramic products in this preferred range, the average drop hammer height is greater than or equal to 25cm.
[0031] The yttria-stabilized zirconia used in the present invention is common yttria-stabilized zirconia in the art and can be purchased commercially. Optionally, the molar ratio of yttria to zirconia contained in the yttria-stabilized zirconia is (1.5-4):(98.5-96).
[0032] Preferably, in the drop weight impact test result of the ceramic, the average drop weight height is greater than or equal to 25 cm, and preferably the average drop weight height is 25-30 cm. It can be seen from this that the ceramic can have high impact resistance. Greater than or equal to 25 cm is a test value for a better drop weight test effect of the ceramic when the ceramic is used as an electronic product.
[0033] According to the present invention, preferably, in the density test result of the ceramic, the average number of pits with a pit diameter greater than 20 μm in every 10×10 mm range is 0. It can be seen that the ceramic has high density and there are no pit defects visible to the naked eye on the ceramic surface.
[0034] Optionally, the sintering temperature required for preparing the ceramic is equal to or less than 1500 degrees Celsius. The lower sintering temperature does not require a high sintering furnace, which is conducive to large-scale industrial production, and the low sintering temperature is conducive to energy conservation and green production.
[0035] A second aspect of the present invention provides a method for preparing a ceramic, comprising:
[0036] (1) adding water, a dispersant and a binder to a powder containing barium oxide, aluminum oxide, yttria-stabilized zirconium oxide and 3Al2O3·2SiO2 (i.e., mullite) and performing wet grinding to obtain a slurry;
[0037] (2) drying the slurry to obtain ceramic powder;
[0038] (3) The ceramic powder is molded and then sintered in air to obtain ceramics.
[0039] Barium oxide and aluminum oxide form BaAl at sintering temperature. 12 O 19 , while 3Al2O3·2SiO2 (i.e. mullite) was not found to change its phase during high temperature sintering.
[0040] The powder contains 6.01-14.02 wt% of barium oxide, 23.98-55.95 wt% of aluminum oxide, 25.34-69.5 wt% of yttria-stabilized zirconium oxide, and 0.5-4.66 wt% of 3Al2O3·2SiO2. Barium oxide and aluminum oxide form BaAl2O3 at the sintering temperature. 12 O 19 However, no phase change was found in 3Al2O3·2SiO2 (i.e., mullite) during high-temperature sintering. The roles of 3Al2O3·2SiO2 and yttria-stabilized zirconia in ceramics are as described above and will not be repeated here.
[0041] In the present invention, barium oxide, aluminum oxide, yttria-stabilized zirconium oxide, and 3Al2O3·2SiO2 (ie, mullite) can be provided in the form of respective powders.
[0042] Preferably, the content of barium oxide is 8.01-12.02wt%, the content of aluminum oxide is 31.97-47.96wt%, the content of yttria-stabilized zirconium oxide is 36-59.33wt%, and the content of 3Al2O3·2SiO2 is 0.67-4wt%. The inventors of the present invention have found through a large number of experiments that in the drop hammer impact test results of the ceramic product prepared within this preferred range, the average drop hammer height is greater than or equal to 25cm.
[0043] Optionally, the molding method is a molding method known to those skilled in the art, and can be one of dry pressing, isostatic pressing, injection molding, and hot die casting. Preferably, dry pressing can be used, and a press with a tonnage of 180-220 tons and an oil pressure of 6-10 MPa can be used for molding, for example, it can be molded into the shape of a mobile phone back cover.
[0044] Optionally, the dispersant is selected from at least one of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose and triethanolamine; the binder is selected from polyvinyl alcohol and / or polyethylene glycol 4000; preferably, the binder is polyvinyl alcohol (PVA) and polyethylene glycol 4000 (PEG4000), and the molar ratio of polyvinyl alcohol to polyethylene glycol 4000 is 1:1-2, preferably 1:1.
[0045] Optionally, the added amount of the dispersant is 0.005-0.5% by weight of the powder, preferably 0.01-0.1% by weight.
[0046] Optionally, the amount of the binder added is 0.5-5% by weight of the powder, preferably 2-5% by weight.
[0047] Preferably, the solid content of the slurry is 20-60% by weight, preferably 25-55% by weight. When the solid content of the slurry is within the above range, better abrasive effect can be achieved.
[0048] The dispersant can promote uniform mixing of the components in the powder. The binder is beneficial to the formability of the powder. In the present invention, the dispersant and the binder can be commercially available.
[0049] In some embodiments, step (1) implements grinding the powders of various oxides used as raw materials to reduce the particle size and obtain a slurry. The grinding process is wet grinding, and the specific process may include: mixing the powders of various oxides and water into a slurry, first ball milling and mixing, and then sand milling to make the median particle size of various oxides reach the nanometer level (such as 250-500nm). More specifically, the various oxides are ball milled in a ball mill according to the content of the present invention for 8-10 hours, and then a dispersant and water are added to a sand mill for sand milling for 8-10 hours, and finally a suitable proportion of a binder (such as PVA and / or polyethylene glycol 4000) is added and stirred for 0.5-4 hours. The ball mill and the sand mill use a zirconia ceramic liner and zirconia grinding balls. The selected particle size of the zirconia grinding balls, the ratio of grinding balls of different particle sizes, the weight ratio of grinding balls to powder, and the amount of water can be controlled to achieve the desired particle size of the oxide.
[0050] In some embodiments, step (2) can be dried in various ways, such as spray drying, to form a spherical powder with strong fluidity. Preferably, the inlet air temperature of the spray drying is 220-280°C, the outlet air temperature is 100-120°C, and the centrifugal speed is 10-20 revolutions per second.
[0051] Preferably, in the embodiment provided by the present invention, the sintering procedure of step (3) includes: heating from room temperature to 600°C over 400 minutes and keeping warm for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping warm for 2 hours, heating from 1150°C to 1400-1500°C over 150 minutes and keeping warm for 1-2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0052] In some embodiments, the ceramic obtained after sintering further includes flat grinding and polishing, and is cut into a final product using a laser.
[0053] The third aspect of the present invention provides a ceramic produced by the preparation method of the present invention.
[0054] The fourth aspect of the present invention provides an application of the ceramic provided by the present invention in preparing an electronic product housing. For example, the electronic product housing may be a mobile phone housing (i.e., a mobile phone back cover), a watch housing, a computer housing, and the like.
[0055] In the present invention, barium oxide, aluminum oxide, yttria-stabilized zirconium oxide, and 3Al2O3·2SiO2 (ie, mullite) can be provided in the form of respective powders.
[0056] In the present invention, step (1) is to grind the various powders used as raw materials to reduce the particle size and obtain a slurry. The grinding process is wet grinding, and the specific process may include: mixing the various powders and water into a slurry, first ball milling and mixing, and then sand milling to make the median particle size of the various powders reach the nanometer level (such as 250-500nm). More specifically, the various powders are ball milled for 8-10 hours in a ball mill according to the content of the present invention, and then a dispersant and water are added to a sand mill for sand milling for 8-10 hours, and finally a suitable proportion of a binder (such as PVA and / or polyethylene glycol 4000) is added and stirred for 2-4 hours. The ball mill and the sand mill use a zirconia ceramic liner and zirconia grinding balls. The selected particle size of the zirconia grinding balls, the ratio of grinding balls with different particle sizes, the weight ratio of grinding balls to powders, and the amount of water can be controlled to achieve the desired particle size of the oxide.
[0057] According to the present invention, in the method provided, various powders are fed to form the powder. The feeding amount of various powders finally meets the composition requirements of the obtained ceramic. In the present invention, in the powder, the total weight of each powder fed is 100 weight%.
[0058] In the present invention, the ceramic obtained by sintering is also subjected to flat grinding and polishing, and is cut into a final product using a laser.
[0059] The present invention will be described in detail below through examples.
[0060] Density: The average number of pits (greater than 20 μm) within 10×10 mm on the large surface of the polished sample
[0061] Drop hammer impact: Use a drop hammer impact tester (manufacturer CKSI, model E602SS), place the sample on the platform, use a 60g drop hammer to hit the center of the sample, starting from a height of 5cm. If there is no crack, increase the height by 5cm each time until visible cracks appear on the sample, and record the height value.
[0062] Average drop hammer height: In the embodiments or comparative examples of the present invention, 10 identical samples are prepared at one time, and the drop hammer impact height is measured 10 times. The average value is taken to obtain the average drop hammer height.
[0063] XRD test: Use Smartlab (3kW) X-ray diffractometer to test the phase type and content.
[0064] XRF detection: Energy dispersive X-ray fluorescence spectrometer EDX-7000 was used to test the element content of the polished samples.
[0065] Dielectric constant test: The dielectric constant is tested at 2 GHz using a dielectric resonator and a resonant cavity method.
[0066] Density test: Use the drainage method to test the density of related products.
[0067] The following are specific examples and comparative examples of the present invention.
[0068] Example 1
[0069] Raw materials: 200g of powder, which contains 10.03wt% of barium oxide (BaO), 39.97wt% of aluminum oxide (Al2O3), 2wt% of 3Al2O3·2SiO2 (i.e., mullite), and 48wt% of yttria-stabilized zirconia powder, wherein the molar ratio of yttria to zirconium oxide in the yttria-stabilized zirconia powder is 3:97.
[0070] The powder was ball-milled in a ball mill for 8 hours with water, and then 0.02 wt% of the powder weight of the dispersant hydroxypropyl methylcellulose and water were added to the sand mill for 10 hours, and finally 4 wt% of the powder weight of the binder was added, the binder was a mixture of PEG4000 and PVA with a molar ratio of 1:1, and stirred for 0.5 hours to form a spray slurry with a solid content of 25 wt%.
[0071] The slurry is sent to a spray tower for spray drying. The spray drying conditions are as follows: the inlet air temperature is 250°C, the outlet air temperature is 110°C, and the centrifugal speed is 15 revolutions per second, forming a spherical powder with strong fluidity for dry pressing. After that, dry pressing is performed. The dry pressing molding conditions are as follows: a 200-ton press machine is used with an oil pressure of 8MPa for dry pressing.
[0072] The molding powder was heated from room temperature to 600°C over 400 minutes and kept warm for 2 hours, then heated from 600°C to 1150°C over 300 minutes and kept warm for 2 hours, then heated from 1150°C to 1430°C over 150 minutes and kept warm for 2 hours, then cooled to 900°C over 150 minutes, and finally naturally cooled to room temperature. The above sintering process was carried out in air.
[0073] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0074] The prepared sample was subjected to high-energy XRF (X-ray fluorescence spectrometry) detection, and the composition elements contained: Zr: 33.9wt%, Y: 2.3wt%, Ba: 9.2wt%, Al: 22.1wt%, and Si: 0.3wt%.
[0075] The phases detected by XRD (X-ray diffraction) include: yttria-stabilized zirconia 47.7wt%, BaAl 12 O 19 It is 50.2wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 2.1wt%.
[0076] Example 2
[0077] Raw materials: 200g of powder, which contains 10.03wt% of barium oxide (BaO), 39.97wt% of aluminum oxide (Al2O3), 3.3wt% of 3Al2O3·2SiO2 (i.e., mullite), and 46.7wt% of yttria-stabilized zirconia powder.
[0078] The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1, and both are commercially available.
[0079] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0080] The molded powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, then heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, then heating from 1150°C to 1400°C over 150 minutes and keeping it for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0081] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0082] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr: 33.1wt%, Y: 2.2wt%, Ba: 9.1wt%, Al: 22.5wt%, and Si: 0.4wt%.
[0083] The phases detected by XRD include: yttria-stabilized zirconia (46.5wt%), BaAl 12 O 19 It is 50.1wt%, and the 3Al2O3·2SiO2 (ie mullite) phase is 3.4wt%.
[0084] Example 3
[0085] Raw materials: 200g of powder, which contains 10.03wt% of barium oxide (BaO), 39.97wt% of aluminum oxide (Al2O3), 0.83wt% of 3Al2O3·2SiO2 (i.e., mullite) powder, and 49.17wt% of yttria-stabilized zirconia powder.
[0086] The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1, and both are commercially available.
[0087] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0088] The molded powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, heating from 1150°C to 1450°C over 150 minutes and keeping it for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0089] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0090] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained 34.8wt% Zr, 2.4wt% Y, 9.2wt% Ba, 21.6wt% Al, and 0.1wt% Si.
[0091] The phases detected by XRD include: yttria-stabilized zirconia (48.8 wt%), BaAl 12 O 19 It is 50.3wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 0.9wt%.
[0092] Example 4
[0093] Raw materials: 200g of powder, which contains 12.03wt% of barium oxide (BaO), 47.97wt% of aluminum oxide (Al2O3), 2.4wt% of 3Al2O3·2SiO2 (i.e., mullite), and 37.6wt% of yttria-stabilized zirconia powder. The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1, and both are commercially available.
[0094] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0095] The formed powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping the temperature for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping the temperature for 2 hours, heating from 1425°C to 1425°C over 150 minutes and keeping the temperature for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0096] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0097] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr: 26.6wt%, Y: 1.9wt%, Ba: 13.1wt%, Al: 26.4wt%, and Si: 0.4wt%.
[0098] The phases detected by XRD include: yttria-stabilized zirconia (37.4 wt%), BaAl 12 O 19 It is 60.1wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 2.5wt%.
[0099] Example 5
[0100] Raw materials: 200 g of powder, which contains 8.02 wt% of barium oxide (BaO), 31.98 wt% of aluminum oxide (Al2O3), 1.6 wt% of 3Al2O3·2SiO2 (i.e., mullite) powder, and 58.4 wt% of yttria-stabilized zirconia powder. The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1 and is commercially available.
[0101] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0102] The formed powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping the temperature for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping the temperature for 2 hours, heating from 1435°C to 1435°C over 150 minutes and keeping the temperature for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0103] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0104] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr: 41.3wt%, Y: 2.8wt%, Ba: 7.4wt%, Al: 17.6wt%, and Si: 0.3wt%.
[0105] The phases detected by XRD include: yttria-stabilized zirconia (58.2 wt%), BaAl 12 O 19 It is 40.1wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 1.7wt%.
[0106] Example 6
[0107] The difference from Example 1 is:
[0108] Raw materials: 200 g of powder, which contains 6wt% of barium oxide (BaO), 24wt% of aluminum oxide (Al2O3), 4.65wt% of 3Al2O3·2SiO2 (i.e., mullite) powder, and 65.35wt% of yttria-stabilized zirconia powder. The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1 and is commercially available.
[0109] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr: 46.3wt%, Y: 3.2wt%, Ba: 5.7wt%, Al: 14.5wt%, and Si: 0.9wt%.
[0110] The phases detected by XRD include: yttria-stabilized zirconia (65.1 wt%), BaAl 12 O 19 It is 30.2wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 4.7wt%.
[0111] Example 7
[0112] The difference from Example 1 is:
[0113] Raw materials: 200 g of powder, which contains 14 wt% of barium oxide (BaO), 56 wt% of aluminum oxide (Al2O3), 0.5 wt% of 3Al2O3·2SiO2 (i.e., mullite) powder, and 29.5 wt% of yttria-stabilized zirconia powder. The chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1 and is commercially available.
[0114] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr: 20.9wt%, Y: 1.5wt%, Ba: 13.4wt%, Al: 29.9wt%, and Si: 0.1wt%.
[0115] The phases detected by XRD include: yttria-stabilized zirconia (29.2 wt%), BaAl 12 O 19 It is 70.2wt%, and the 3Al2O3·2SiO2 (i.e. mullite) phase is 0.6wt%.
[0116] Comparative Example 1
[0117] Raw materials: 200g of powder, which contains 50wt% of aluminum oxide (Al2O3) and 50wt% of yttria-stabilized zirconia powder, the chemical composition of which is the same as that of Example 1 and is commercially available. The powder is an existing combination for preparing ceramics with relatively low density.
[0118] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0119] The formed powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping the temperature for 2 hours, then heating from 600°C to 1150°C over 300 minutes and keeping the temperature for 2 hours, then heating from 1150°C to 1600°C over 150 minutes and keeping the temperature for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0120] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0121] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr was 35.3wt%, Y was 2.4wt%, and Al was 26.6wt%.
[0122] The phases detected by XRD include: yttria-stabilized zirconia accounting for 49.9wt% and Al2O3 accounting for 50.1wt%.
[0123] Comparative Example 2
[0124] Raw materials: 200 g of powder, 100 wt % of yttria-stabilized zirconia powder, the chemical composition of the yttria-stabilized zirconia powder is the same as that of Example 1, and both are commercially available.
[0125] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0126] The molded powder was sintered in air by heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, heating from 1150°C to 1450°C over 150 minutes and keeping it for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0127] The sintered product is ground, polished and laser cut to produce the final sample, which has the shape and size of a mobile phone back cover, 150*75*0.6mm.
[0128] The prepared sample was subjected to high-energy XRF detection, and the composition elements contained: Zr was 70.3wt% and Y was 4.3wt%.
[0129] The physical phases detected by XRD include: yttria-stabilized zirconia accounting for 100wt%.
[0130] Comparative Example 3
[0131] Raw materials: 200 g of powder containing 10.03 wt % of barium oxide (BaO), 39.97 wt % of aluminum oxide (Al2O3), and 50 wt % of yttria-stabilized zirconium oxide powder containing 3 mol % of yttria. The chemical composition of the yttria-stabilized zirconium oxide powder is the same as that in Example 1 and both are commercially available.
[0132] The wet grinding, drying and molding conditions were the same as those in Example 1 to obtain a molded powder.
[0133] The formed body is sintered in air by heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, heating from 1150°C to 1630°C over 150 minutes and keeping it for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0134] The sintered ceramics were ground and polished and laser cut to a size of 150*75*0.6 mm to obtain ceramic products.
[0135] The product was tested by XRF and XRD, and the results were:
[0136] The constituent elements of the product include: Zr: 35.3wt%, Y: 2.2wt%, Ba: 9.1wt%, and Al: 21.3wt%.
[0137] The product phases include: yttria stabilized zirconia 49.7wt%, BaAl 12 O 19 It is 50.3wt%.
[0138] Comparative Example 4
[0139] The difference from Comparative Example 3 is that the sintering temperature is different:
[0140] The formed body is sintered in air by heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, heating from 1150°C to 1430°C over 150 minutes and keeping it for 2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
[0141] (4) The sintered ceramics are ground and polished and laser cut to a size of 150*75*0.6 mm to obtain ceramic products.
[0142] The product was tested by XRF and XRD, and the results were:
[0143] The constituent elements of the product include: Zr: 35.3wt%, Y: 2.2wt%, Ba: 9.1wt%, and Al: 21.3wt%.
[0144] The product phases include: yttria stabilized zirconia 49.7wt%, BaAl 12 O 19 It is 50.3wt%.
[0145] In addition, it should be noted that, in the XRD test of the present invention, there will normally be a certain test error. For example, in Example 1 of the present invention, the 3Al2O3·2SiO2 (i.e., mullite) phase is 2.1wt%, instead of 2wt% when added. The inventors of the present invention believe that the reason for the slight difference between these two values is the test error. The inventors of the present invention believe that 3Al2O3·2SiO2 (i.e., mullite) does not change under high-temperature sintering. At high temperatures, the synthesis reaction between barium oxide and aluminum oxide forms BaAl 12 O 19 , while 3Al2O3·2SiO2 and yttria-stabilized zirconia did not undergo a synthesis reaction.
[0146] The examples of the present invention and the comparative examples were tested, and the test results are shown in Table 1.
[0147] Table 1
[0148]
[0149] It can be seen from Table 1 that, compared with Example 1 and Comparative Example 1, the ceramic prepared by Example 1 using the technical solution of the present invention has a significantly improved average drop hammer height, i.e., impact resistance, compared with the ceramic with reduced density disclosed in Comparative Example 1, and the sintering temperature is greatly reduced. Compared with Comparative Example 2, i.e., completely yttria-modified zirconia, Example 1 of the present invention has a reduced dielectric constant, which is beneficial to the stable transmission of electrical signals when it is applied to electronic products, and the density is reduced, making the prepared ceramic product lighter, meeting the product optimization requirements when applied to electronic products. Compared with Comparative Example 3 without mullite, Example 3 of the present invention has a significantly reduced sintering temperature, and the average drop hammer height, i.e., impact resistance, is slightly improved, indicating that mullite can significantly reduce the sintering temperature and is beneficial to further improve the impact resistance to a certain extent. Compared with Example 4, Example 1 of the present invention does not add mullite in Example 4, has the same sintering temperature as Example 1, and has the same ingredients as Example 3. The sintering temperature is lower than that of Example 3. The ceramic obtained in Example 4 has a poor appearance, a large number of pits on the surface, a lower density than that of Example 3, and lower impact resistance, indicating that the sintering temperature of the ceramic is not enough, resulting in poor density of the product, and further failing to meet the requirements of qualified products in some performance aspects. Therefore, it is explained that the appropriate sintering temperature of the powders of Examples 3 and 4 is 1630 degrees Celsius, but such a high temperature requirement is not conducive to large-scale mass production.
[0150] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a ceramic, It is characterized in that include: (1) Containing barium oxide, aluminum oxide, yttria-stabilized zirconium oxide, 3Al 2 O 3 ·2SiO 2 The powder is wet-milled with water, a dispersant and a binder to obtain a slurry; (2) drying the slurry to obtain ceramic powder; (3) forming the ceramic powder, and then sintering it in air to obtain a ceramic, The ceramic phase contains: 40-60wt% BaAl 12 O 19 , 0.67-4wt% 3Al 2 O 3 ·2SiO 2 , 36-59.33wt% yttria stabilized zirconia, The sintering procedure includes: heating from room temperature to 600°C over 400 minutes and keeping it for 2 hours, heating from 600°C to 1150°C over 300 minutes and keeping it for 2 hours, heating from 1150°C to 1400-1500°C over 150 minutes and keeping it for 1-2 hours, then cooling to 900°C over 150 minutes, and finally naturally cooling to room temperature.
2. The preparation method according to claim 1, It is characterized in that In the drop weight impact test results of the ceramic, the average drop weight height is greater than or equal to 25 cm.
3. The preparation method according to claim 1, It is characterized in that In the density test results of the ceramic, the average number of pits with a pit diameter greater than 20 μm within a range of 10×10 mm is 0.
4. The preparation method according to claim 1, It is characterized in that The powder contains 6.01-14.02wt% barium oxide, 23.98-55.95wt% aluminum oxide, 25.34-69.5wt% yttria-stabilized zirconium oxide, and 3Al 2 O 3 ·2SiO 2 The content is 0.5-4.66wt%.
5. The preparation method according to claim 4, It is characterized in that The content of barium oxide is 8.01-12.02wt%, the content of aluminum oxide is 31.97-47.96wt%, the content of yttria-stabilized zirconium oxide is 36-59.33wt%, 3Al 2 O 3 ·2SiO 2 The content is 0.67-4wt%.
6. The preparation method according to claim 1, It is characterized in that In the powder, the molar ratio of yttria to zirconium oxide contained in the yttria-stabilized zirconium oxide is (1.5-4): (98.5-96).
7. The preparation method according to claim 1, It is characterized in that The molding is performed by one of dry pressing, isostatic pressing, injection molding, and hot die casting.
8. The preparation method according to claim 1, It is characterized in that In step (1), the dispersant is selected from at least one of hydroxypropyl methylcellulose, sodium carboxymethyl cellulose and triethanolamine; the binder is selected from polyvinyl alcohol and / or polyethylene glycol 4000; The dispersant is added in an amount of 0.005-0.5% by weight of the powder; The amount of the binder added is 0.5-5% by weight of the powder; The solid content of the slurry is 20-60% by weight.
9. The preparation method according to claim 8, It is characterized in that The added amount of the dispersant is 0.01-0.1% by weight of the powder.
10. The preparation method according to claim 8, It is characterized in that The amount of the binder added is 2-5% by weight of the powder.
11. The preparation method according to claim 8, It is characterized in that The solid content of the slurry is 25-55% by weight.
12. A ceramic obtained by the preparation method according to any one of claims 1 to 11.
13. Use of the ceramic according to claim 12 in preparing electronic product housings.
Citation Information
Patent Citations
Thermal shock-resistant composite materials