A curable composition and its application
By preparing liquid polythiol compounds with specific ion content combined with epoxy resin to form a curable composition, the problem of aging and degradation of the adhesive is solved, the service life is extended and the performance is improved, and the appearance and strength of the adhesive is ensured.
Patent Information
- Application Number
- CN202311270082.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-09-28
AI Technical Summary
During storage, existing adhesives are easily affected by light, heat, oxygen and metal ions, resulting in aging and degradation, affecting their appearance, strength and service life, and the impact of ion content in thiol on adhesive performance has not been fully studied. .
By preparing a liquid polythiol compound, reacting polyols and halogenated hydrocarbons to form a polymer with two or more thiol groups, and thiolization is carried out under high temperature and high pressure conditions, the ion content of Ba, Ni, and Sn is controlled to be 50ppm-5 Within the range of %, a curable composition is formed in combination with an epoxy resin and an accelerator for the preparation of an adhesive.
Effectively control the curing time of the adhesive to ensure that its strength remains unabated, its appearance is complete, its transmittance is high, its haze is low, it prolongs its service life, and avoids performance degradation caused by excessive or low ion content.
Smart Images

Figure BDA0004475328820000071 
Figure BDA0004475328820000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to a curable composition and application thereof. Background Art
[0002] There are many types of epoxy resin curing agents, such as amines, anhydrides, synthetic resins, etc., which are currently widely used in the fields of fast adhesives, potting, lamination, casting, coatings, and silicon rod cutting adhesives. However, these curing agents have the disadvantage of high curing temperatures and cannot be used in low temperature environments. Polythiol epoxy resin curing agents can be quickly cured in 5 to 10 minutes at -20 to 20°C and in a humid environment. Due to its excellent performance, it is gradually replacing traditional epoxy resin curing agents.
[0003] Polythiol curing agent is a low-temperature fast epoxy curing agent used in recent years. Its terminal group has more than two -SH groups and is mainly used for room temperature curing of epoxy resin. Compared with other epoxy curing agents, it has significant advantages such as low curing temperature, rapid curing, thin layer curing and light color, and is a product that cannot be replaced by other types of curing agents. At the same time, due to the presence of sulfur flexible segments and high refractive index, it also has great application value in toughening resins and transparent resins.
[0004] In recent years, with the emergence of various new adhesive materials, bonding technology has been increasingly widely used in defense, aerospace, precision electronics, high-end optical materials, historical relics restoration, and jewelry restoration. Practice has shown that the bonding interface will be affected by light, heat, oxygen, and metal ions during storage, causing aging and degradation, which will affect its appearance, adhesive layer strength, and service life. Li Ailing and others studied the durability of polyurethane adhesives in sodium chloride aqueous solution. Davis Fata and others studied the effects of thermal aging and hydrothermal aging changes on epoxy adhesives, etc.
[0005] However, there is still no relevant literature or technical disclosure on the effect of the ion content in the mercaptan on the aging performance of the adhesive. Summary of the invention
[0006] In view of the problems of the prior art, the inventors found in the research process that some ion contents in the polythiol compound will affect the curing time, adhesive strength, transmittance, haze, etc. of the adhesive. Therefore, through further research, the present invention provides a liquid polythiol compound, and further provides its application in the preparation of adhesives. Through the technical scheme of the present invention, the curing time of the adhesive prepared by it can be effectively controlled, and the self-curing time is about 3-15min, which does not affect its strength, and the synthesized adhesive material has a complete and flawless appearance, high transmittance, and low haze.
[0007] In order to achieve the above technical effects, the technical solution of the present invention is as follows:
[0008] Firstly, the present invention provides a liquid polythiol compound, which is obtained by reacting a polyol, a halogenated hydrocarbon and a thiol-forming agent, wherein each molecule contains two or more thiols, and the total content of Ba, Ni and Sn in the polymer is 50ppm-5%.
[0009] Preferably, the total content of Ba, Ni and Sn in the polythiol compound is 100 ppm-1%.
[0010] The specific preparation method of the liquid polythiol compound is:
[0011] The polyol and the halogenated hydrocarbon react at a temperature of 20-90°C for 1-10 hours under the action of a catalyst. After the reaction is completed, a phase transfer catalyst and a thiol reagent are added, and the thiol reaction is carried out under high temperature, high pressure and protective gas conditions for a reaction time of 0.5-10 hours to generate a polythiol compound. After the reaction is completed, the aqueous phase is removed, and water washing and acid washing are performed, and then the liquid is separated, and the polythiol product is obtained by rotary evaporation. The Ba, Ni, and Sn ion contents in the polythiol product are determined, and the total amount of Ba, Ni, and Sn ions is adjusted to the corresponding range by adding compounds of the corresponding elements.
[0012] Preferably, the Sn compound is selected from any one or more of dimethyltin mercaptide, dimethyltin, butyltin carboxylate, and octyltin mercaptide; the Ba compound is BaSO 4 ;Ni compound is nickel sulfate.
[0013] The polyol is selected from polyether polyols using glycerol as an initiator, and has a hydroxyl value of 300-600 mgKOH / g.
[0014] The molar ratio of the halogenated hydrocarbon to the polyol is (0.6-5):1, preferably (1-3):1.
[0015] Preferably, the halogenated hydrocarbon is epichlorohydrin.
[0016] The catalyst is selected from tin tetrachloride, stannous octoate, tributyltin chloride, etc. The amount of the catalyst is 0.1%-5% of the mass of the polyol, preferably 0.5%-3%.
[0017] The reaction temperature of the polyol and the halogenated hydrocarbon is preferably 30-70° C.; the reaction time is preferably 3-7 hours.
[0018] The thiol-forming agent is selected from one of sodium hydrosulfide, thiourea, sodium sulfide, sodium polysulfide, etc., preferably one of sodium hydrosulfide, sodium polysulfide, and thiourea.
[0019] The molar ratio of the thiol-forming agent to the halogenated hydrocarbon is (2-8):1, preferably (3-5):1.
[0020] The reaction temperature of the thiolation reaction is specifically 70-150° C., and the reaction pressure is 0.1-10 MPa; the preferred reaction temperature is 90-120° C., and the reaction pressure is 0.5-5 MPa.
[0021] The reaction time of the thiolation reaction is preferably 3-6 hours.
[0022] The protective gas is selected from CO 2 , nitrogen, argon, hydrogen sulfide, etc., preferably nitrogen or hydrogen sulfide.
[0023] The phase transfer catalyst is selected from tetrabutylammonium chloride, tetrabutylammonium bromide, benzyltriethylammonium chloride, polyethylene glycol, glycerol, crown ether, and tertiary amine, preferably tetrabutylammonium bromide or polyethylene glycol. The amount of the phase transfer catalyst is 1%-25% of the mass of the polyol, preferably 5%-10%.
[0024] After obtaining the above-mentioned liquid polythiol compound, the present invention further provides a curable composition, which comprises: the above-mentioned liquid polythiol compound, an epoxy resin and an accelerator; in parts by weight, the liquid polythiol compound is 10-90 parts, the epoxy resin is 10-90 parts, and the accelerator is 0.1-15 parts.
[0025] Preferably, in parts by weight, the contents of the components in the composition are: 30-60 parts of liquid polythiol compound, 30-60 parts of epoxy resin, and 2-9 parts of accelerator.
[0026] The epoxy resin is selected from one or two of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, epoxidized olefin epoxy resin, hydantoin epoxy resin, imide epoxy resin, silicone epoxy resin, and organoferric epoxy resin. Preferably, it is one or a combination of glycidyl ether epoxy resin and glycidyl ester epoxy resin.
[0027] The accelerator is selected from ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,5-diaminopentane, hexamethylenediamine, tetramethylenediamine, trimethylhexamethylenediamine, 2-methyl-1,5-diaminopentane, polyetherdiamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, diethylenepropylamine, polyamide, isophoronediamine, N-aminoethylpiperazine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, m-phenylenediamine, dicyandiamide, adipic acid dihydrazide, dipropylenetriamine, bis(hexamethylene)triamine, 2,4,6-tri(di The accelerators include 2,4,6-tris(dimethylaminomethylphenol), 2,4,6-tris(dimethylaminomethylphenol) tris(2-ethylhexanoate), 2,4,6-tris(dimethylaminomethylphenol) trioleate, benzyldimethylamine, ethylenediamine, triethanolamine, o-hydroxybenzyldimethylamine, acetylacetonate metal salts, triphenylphosphine and its phosphonate, active tris(2-ethylhexanoate)chromium, organic acid salt amine complex, 1,8-diaza-bicyclo(5,4,0)-7-undecene, 2-thiolbenzothiazole, thiourea and its derivatives, cycloalkylimidazoline, 2-imidazoline, aromatic tertiary amine containing epoxy group, phthalate accelerator, etc. Preferably, the accelerators include 2,4,6-tris(dimethylaminomethylphenol), benzyldimethylamine, ethylenediamine, triethanolamine, o-hydroxybenzyldimethylamine, triphenylphosphine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine.
[0028] The components of the curable composition described in the present invention are stored separately, or the liquid polythiol compound and the accelerator are mixed and stored, and the epoxy resin is stored separately, and then mixed according to the ratio when used; when applied to AB glue, the epoxy resin in a proportional amount is added to the A component, and the liquid polythiol compound and the accelerator are added to the B component.
[0029] In summary, the present invention provides a liquid polythiol compound, and further provides a curable composition. The adhesive prepared with the composition can effectively solve the problem of long-term aging degradation, thereby extending its service life. When the ion content is within the specified range of the present invention, the synthesized adhesive material has a complete and flawless appearance, high transmittance, and low haze. When the ion content is lower than the specified range of the present invention, it will cause the polymerization rate of the composition to accelerate and the cross-linking density to be low, thereby affecting the strength of the adhesive. When the ion content exceeds the specified range of the present invention, the adhesive material has a low appearance transmittance and high haze, which affects the qualified rate of the finished product. DETAILED DESCRIPTION
[0030] The following is a further detailed description of the above contents of the present invention through specific implementation methods in the form of examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention, and unless otherwise specified, the raw materials used in the following examples are all commercially available products.
[0031] In order to further illustrate the present invention, the following examples are provided for detailed description.
[0032] 1. Determination of ion content
[0033] Inductively coupled plasma optical emission spectrometry was used to determine the ion content in polythiol compounds.
[0034] 2. Transmittance measurement
[0035] The test was conducted using the American HunterLab UltraScan PRO spectrophotometer.
[0036] 3. Determination of haze value
[0037] The test was conducted using the American HunterLab UltraScan PRO spectrophotometer.
[0038] 4. Anti-aging evaluation test, using Q-LAB SPRAY UV aging box to simulate UV irradiation λ = 340nm, 0.75mW / cm 2 , observe the surface state and transparency of the solidified material after different times.
[0039] Synthesis example 1
[0040] Add 150 g of polyol (R2302 from Yantai Wanhua Chemical) and 0.75 g of catalyst SnCl into the reaction vessel. 4 ·5H 2 O, start stirring and heating, raise the temperature to 100℃; slowly add 147g of epichlorohydrin (99.5%) dropwise for about 1h. After the addition is complete, keep the temperature at 40℃ for 2h, then add 241g of NaHS solution (44wt%) and 15g of tetrabutylammonium chloride in sequence, fill with protective gas H 2 S (pressure 0.5Mpa), keep the reaction at 100℃ for 5h.
[0041] After the reaction, the aqueous phase was removed, 900 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic (pH 3-5), stirred for 5 hours, allowed to stand for separation, and then 900 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.41 g of polythiol product was obtained by rotary evaporation.
[0042] The Sn content in the polythiol product was detected to be 30 ppm, and then 0.0047 g of BaSO was added. 4 The mixture was stirred with 0.0073 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0043] Synthesis example 2
[0044] Add 150g of polyol (Bluestar Dongda MN-500) and 1.13g of catalyst stannous octoate to the reaction vessel, start stirring and heating, and raise the temperature to 100°C; slowly add 113g of epichlorohydrin (99.5%) to the bottle, and the addition time is about 1h. After the addition is completed, keep it warm at 70°C for 4h, add 332g of NaHS solution (32wt%) and 18g of glycerol in turn, fill with protective gas N2 (pressure 0.6Mpa), and keep it warm at 90°C for 7h.
[0045] After the reaction, the aqueous phase was removed, 600 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic (pH 3-5), stirred for 5 hours, allowed to stand for separation, and then 600 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.38 g of polythiol product was obtained by rotary evaporation.
[0046] The Sn content in the polythiol product was detected to be 50 ppm, and then 0.017 g of BaSO was added. 4 The mixture was stirred with 0.018 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0047] Synthesis example 3
[0048] Add 150g polyol (Nantong Chenrun GP-303) and 1.5g catalyst tributyltin chloride to the reaction vessel, start stirring and heating, and raise the temperature to 100°C; slowly drop 102g epichlorohydrin (99.5%) into the bottle, and the drop time is about 1h. After the dropwise addition is completed, keep warm at 60°C for 1h, add 322g NaHS solution (33wt%) and 25g tetrabutylammonium bromide in turn, fill with protective gas H2S (pressure 0.3Mpa), and keep warm at 110°C for 3h.
[0049] After the reaction, the aqueous phase was removed, 300 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic (pH 3-5), stirred for 5 hours, allowed to stand for separation, and then 300 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.69 g of the polythiol product was obtained by rotary evaporation.
[0050] The Sn content in the polythiol product was detected to be 100 ppm, and then 8.32 g of methyltin mercaptan and 1.11 g of BaSO were added. 4 The mixture was stirred with 1.83 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0051] Synthesis example 4
[0052] Add 150 g of polyol (Yinoway New Material C305) and 0.6 g of catalyst SnCl into the reaction vessel. 4 ·5H 2O, start stirring and heating, raise the temperature to 100℃; slowly add 124g of epichlorohydrin (99.5%) to the bottle, the addition time is about 1h. After the addition is completed, keep it at 50℃ for 3h, add 590.27g of NaHS solution (18wt%) and 13.7g of tetrabutylammonium chloride in sequence, fill with protective gas CO 2 (pressure 0.6Mpa), keep the reaction at 120℃ for 2h.
[0053] After the reaction, the aqueous phase was removed, 200 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic (pH 3-5), stirred for 5 hours, allowed to stand for separation, and then 200 g of water was added to the organic phase, washed with water for 5 hours, separated, and 269.89 g of polythiol product was obtained by rotary evaporation.
[0054] The Sn content in the polythiol product was detected to be 100 ppm, and then 52.70 g of methyltin mercaptan and 4.72 g of BaSO were added. 4 The mixture was stirred with 7.21 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0055] Synthesis example 5
[0056] Add 150 g of polyol (R2302 from Yantai Wanhua Chemical) and 0.75 g of catalyst SnCl into the reaction vessel. 4 ·5H 2 O, start stirring and heating, raise the temperature to 100℃; slowly add 147g of epichlorohydrin (99.5%) dropwise for about 1h. After the addition is complete, keep the temperature at 40℃ for 2h, then add 241g of NaHS solution (44wt%) and 15g of tetrabutylammonium chloride in sequence, fill with protective gas H 2 S (pressure 0.5Mpa), keep the reaction at 100℃ for 5h.
[0057] After the reaction, the aqueous phase was removed, 500 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic (pH 3-5), stirred for 5 hours, allowed to stand for separation, and then 500 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.1 g of polythiol product was obtained by rotary evaporation.
[0058] The Sn content in the polythiol product was detected to be 100 ppm.
[0059] Synthesis example 6
[0060] Add 150g of polyol and 0.75g of catalyst SnCl into the reaction vessel. 4 .5H 2O, start stirring and heating, raise the temperature to 100℃; slowly add 147g of epichlorohydrin (99.5%) to the bottle, the addition time is about 1h. After the addition is completed, keep it at 40℃ for 2h, add 241g NaHS solution (44wt%) and 15g tetrabutylammonium chloride, fill with protective gas H 2 S (pressure 0.5Mpa), keep the reaction at 100℃ for 5h.
[0061] After the reaction, the aqueous phase was removed, 250 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic, stirred for 5 hours, allowed to stand for separation, and then 250 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.09 g of the polythiol product was obtained by rotary evaporation.
[0062] The Sn content in the polythiol product was detected to be 100 ppm, and then 17.48 g of octyltin mercaptan was added and stirred at 50° C. for 1 hour, and the temperature was lowered for detection.
[0063] Comparative Synthesis Example 1
[0064] Add 150g of polyol and 0.75g of catalyst SnCl into the reaction vessel. 4 .5H 2 O, start stirring and heating, raise the temperature to 100℃; slowly add 147g of epichlorohydrin (99.5%) to the bottle, the addition time is about 1h. After the addition is completed, keep it at 40℃ for 2h, add 1200g NaHS solution (44wt%) and 15g tetrabutylammonium chloride, fill with protective gas H 2 S (pressure 0.5Mpa), keep the reaction at 100℃ for 5h.
[0065] After the reaction, the aqueous phase was removed, 1200 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic, stirred for 5 hours, allowed to stand for separation, and then 1200 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.24 g of the polythiol product was obtained by rotary evaporation.
[0066] The Sn content in the polythiol product was detected to be 6 ppm, and then 8.32 g of BaSO was added. 4 The mixture was stirred with 14.7 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0067] Comparative Synthesis Example 2
[0068] Add 150g of polyol and 0.75g of catalyst SnCl into the reaction vessel. 4 .5H 2O, start stirring and heating, raise the temperature to 100℃; slowly add 147g of epichlorohydrin (99.5%) to the bottle, the addition time is about 1h. After the addition is completed, keep it at 40℃ for 2h, add 1200g NaHS solution (44wt%) and 15g tetrabutylammonium chloride, fill with protective gas H 2 S (pressure 0.5Mpa), keep the reaction at 100℃ for 5h.
[0069] After the reaction, the aqueous phase was removed, 180 g of water was added to the organic phase, and then dilute hydrochloric acid was added to adjust the pH to acidic, stirred for 5 hours, allowed to stand for separation, and then 180 g of water was added to the organic phase, washed with water for 5 hours, separated, and 277.3 g of polythiol product was obtained by rotary evaporation.
[0070] The Sn content in the polythiol product was detected to be 100 ppm, and then 69.35 g of octyltin mercaptan and 4.72 g of BaSO were added. 4 The mixture was stirred with 7.21 g of nickel sulfate at 50°C for 1 h and then tested by cooling.
[0071] Composition Example 1
[0072] At 25°C and 50% RH, 50g of liquid polythiol compound (Synthesis Example 1) and 2.5g of 2,4,6-tris(dimethylaminomethylphenol) were mixed, and then 50g of epoxy resin E51 was added, and premixed for 20s using a spatula, and then degassed, and the mixture was poured into a mold, and allowed to stand for 3-15min. After complete curing, a cured product with a diameter of 8cm and a thickness of 0.8cm was obtained. The cured product was placed in a Q-LAB SPRAY UV aging box to simulate UV light conditions, and the appearance of the cured product after 7 days and 30 days was observed and tested.
[0073] Composition Examples 2-6
[0074] While keeping other conditions unchanged, the polythiol compounds in composition example 1 are replaced by the polythiol products in synthesis examples 2-6, the epoxy resins are replaced in the order of the examples as follows: E51, E51, E44, E51, E44, and the accelerators are replaced in the order of the examples as follows: 2,4,6-tris(dimethylaminomethylphenol), benzyldimethylamine, benzyldimethylamine, diethylenetriamine, triethylenetetramine, to prepare a cured product.
[0075] Composition Comparative Example 1-2
[0076] With other conditions unchanged, the polythiol compound in Composition Example 1 was replaced by the polythiol products in Synthesis Comparative Examples 1-2, respectively, to prepare cured products.
[0077] The final product performance of each embodiment and comparative example is shown in Table 1 below:
[0078] Table 1 Data table of examples and comparative examples
[0079]
[0080] Composition Examples 5-6
[0081] The preparation method is the same as that of composition Example 1, except that the polythiol compound in Example 1 is replaced by the polythiol compound of Synthesis Example 2, the epoxy resin is replaced by E44, and the accelerator is replaced by diethylenetriamine and benzyldimethylamine in the order of the examples. Other differences are detailed in the following table:
[0082]
[0083] The above embodiments enable those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A liquid polythiol compound, characterized in that: The liquid polythiol compound is obtained by the reaction of a polyol, a halogenated hydrocarbon and a thiol-forming agent, and each molecule contains two or more thiol groups. The Sn content in the polymer is 100ppm-1% or the total content of Ba, Ni and Sn in the polymer is 50ppm-5%, and the content of each Ba, Ni and Sn is not 0.
2. The liquid polythiol compound according to claim 1, characterized in that The total content of Ba, Ni and Sn in the polythiol compound is 100ppm-1%.
3. The liquid polythiol compound according to claim 1, characterized in that The specific preparation method of the liquid polythiol compound is: The polyol and the halogenated hydrocarbon react under the action of a catalyst at a temperature of 20-90°C for 1-10 hours. After the reaction is completed, a phase transfer catalyst and a thiol reagent are added, and a thiol reaction is carried out under high temperature, high pressure and protective gas conditions for a reaction time of 0.5-10 hours to generate a polythiol compound. After the reaction is completed, the aqueous phase is removed, and water washing and acid washing are carried out, and then the liquids are separated, and a polythiol product is obtained by rotary evaporation. The Ba, Ni and Sn ion contents in the polythiol product are determined, and the total amount of Ba, Ni and Sn ions is adjusted to a corresponding range by adding compounds of corresponding elements.
4. The liquid polythiol compound according to claim 3, characterized in that The Sn compound is selected from any one or more of dimethyltin mercaptan, dimethyltin, butyltin carboxylate, and octyltin mercaptan; the Ba compound is BaSO4; and the Ni compound is nickel sulfate.
5. The liquid polythiol compound according to claim 1 or 3, characterized in that: The polyol is selected from polyether polyols using glycerol as an initiator, and the hydroxyl value is 300-600 mgKOH / g; the molar ratio of the halogenated hydrocarbon to the polyol is (0.6-5):
1.
6. The liquid polythiol compound according to claim 3, characterized in that The halogenated hydrocarbon is epichlorohydrin; the catalyst is selected from tin tetrachloride, stannous octoate, and tributyltin chloride; the thiolating agent is selected from one of sodium hydrosulfide, thiourea, sodium sulfide, and sodium polysulfide; the phase transfer catalyst is selected from one of tetrabutylammonium chloride, tetrabutylammonium bromide, benzyltriethylammonium chloride, polyethylene glycol, glycerol, crown ether, and tertiary amine; and the protective gas is selected from one or more of CO2, nitrogen, argon, and hydrogen sulfide.
7. The liquid polythiol compound according to claim 3, characterized in that The amount of the catalyst is 0.1%-5% of the mass of the polyol; the reaction temperature of the polyol and the halogenated hydrocarbon is 30-70°C; the molar ratio of the thiolation agent to the halogenated hydrocarbon is (2-8):1; the reaction temperature of the thiolation reaction is specifically 70-150°C, and the reaction pressure is 0.1-10MPa; the reaction time of the thiolation reaction is 3-6h; the amount of the phase transfer catalyst is 1%-25% of the mass of the polyol.
8. A curable composition, characterized in that The composition comprises the liquid polythiol compound according to claim 1, epoxy resin and accelerator; in parts by weight, the liquid polythiol compound is 10-90 parts, the epoxy resin is 10-90 parts and the accelerator is 0.1-15 parts.
9. The curable composition according to claim 8, characterized in that In terms of weight, the contents of the components in the composition are: 30-60 parts of liquid polythiol compound, 30-60 parts of epoxy resin, and 2-9 parts of accelerator.
10. The curable composition according to claim 8 or 9, characterized in that: The epoxy resin is selected from one or two of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, alicyclic epoxy resin, epoxidized olefin epoxy resin, hydantoin epoxy resin, imide epoxy resin, and silicone epoxy resin; The accelerator is selected from ethylenediamine, 1,2-diaminopropane, 1,3-diaminopropane, 1,5-diaminopentane, hexamethylenediamine, tetramethylenediamine, trimethylhexamethylenediamine, 2-methyl-1,5-diaminopentane, polyetherdiamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, diethylenepropylamine, polyamide, isophoronediamine, N-aminoethylpiperazine, meta-phenylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, meta-phenylenediamine, dicyandiamide, adipic acid dihydrazide, dipropylenetriamine, bis(hexamethylene)triamine, 2,4, 6-Tris(dimethylaminomethylphenol), 2,4,6-tris(dimethylaminomethylphenol) tris(2-ethylhexanoate), 2,4,6-tris(dimethylaminomethylphenol) trioleate, benzyldimethylamine, triethanolamine, o-hydroxybenzyldimethylamine, acetylacetone metal salts, triphenylphosphine and its phosphonium salts, active tris(2-ethylhexanoate) chromium, organic acid salt amine complex, 1,8-diaza-bicyclo(5,4,0)-7-undecene, 2-thiolbenzothiazole, thiourea, cycloalkylimidazoline, 2-imidazoline, aromatic tertiary amines containing epoxy groups, and phthalate accelerators.