Ferroelectric micro-nanocrystalline glass, preparation and application

The preparation of ferroelectric micro-nano crystal glass in one step is solved, and the problem of low crystallinity of ferroelectric micro-crystalline glass in the prior art is achieved efficiently preparing materials with high transparency and high nonlinear optical properties, which are suitable for a variety of applications.

CN117401906BActive Publication Date: 2024-11-22XI AN JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311401676.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-26
Publication Date
2024-11-22
Estimated Expiration
2043-10-26

AI Technical Summary

Technical Problem

In the prior art, the preparation method of ferroelectric crystal glass mainly uses heat treatment to crystallize, resulting in crystals mainly precipitation on the surface, with low crystallinity, making it difficult to regulate and achieve batch preparation of high crystallinity and total homogeneity.

Method used

Using a one-step melting preparation method of tellurate glass and PMN-PT crystal, the PMN-PT crystal is doped at high temperature of 700-900℃ and when the temperature is reduced to 550-600℃, the softening of tellurate glass is combined with low softening of tellurate glass. The temperature and high melting point of PMN-PT crystals achieve efficient preparation of ferroelectric micro-nano crystal glass.

Benefits of technology

It realizes high crystallinity and transparency of ferroelectric micro-nano crystal glass, suitable for nonlinear optical and dielectric materials, combines the resistance to electric breakdown of glass and the dielectric energy storage characteristics of ferroelectric crystals, and is suitable for energy storage capacitors and optical modulator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117401906B_ABST
    Figure CN117401906B_ABST
Patent Text Reader

Abstract

A ferroelectric micro-nano crystalline glass, preparation method and application thereof. The matrix glass material is a tellurite glass of 70TeO2-(10+x)ZnO-(20-x)Na2O (0<x<10), and the doped crystal material is (1-y)Pb(Mg 1 / 3Nb 2 / 3 )O3-yPbTiO3 (0.4
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of novel functional glass materials, and particularly relates to a ferroelectric micro-nano crystalline glass, its preparation and application. Background Art

[0002] Ferroelectric materials are materials with ferroelectric effects and have extensive applications in the fields of electricity, optics, magnetics, etc. With the progress of technology, the development prospects of ferroelectric materials are becoming more and more broad. In terms of electricity, ferroelectric materials can be used to manufacture novel storage devices, such as ferroelectric memories and random access memories, which have the advantages of high speed, low power consumption, high reliability, etc.; ferroelectric materials can also be used to manufacture devices such as ferroelectric sensors and ferroelectric controllers to achieve intelligent control. In terms of optics, ferroelectric materials can be used to manufacture displays such as ferroelectric liquid crystal displays and organic light-emitting diodes, which have the advantages of wide viewing angle, low power consumption, bright colors, etc.; in addition, ferroelectric materials are also expected to be used to manufacture devices such as modulators, lasers and sensors integrated with ferroelectric optical fibers to achieve high-precision, broadband, high-speed communication and measurement.

[0003] PMN-PT is a relaxor ferroelectric crystal material and has currently been widely applied in the fields of piezoelectric materials and devices such as medical ultrasonic probes and marine sonar torpedoes. In recent years, PMN-PT single crystals have been reported to have high transparency and high piezoelectric properties after AC polarization, and at the same time have excellent electro-optic modulation properties and nonlinear optical properties, which have included high-performance piezoelectric crystals in the ranks of optical devices and opened the door to the design of novel acoustic-optic-electric devices (Qiu C, Wang B, Zhang N, et al. Transparent ferroelectric crystals with ultrahigh piezoelectricity [J]. Nature, 2020, 577: 350-354). However, there have been few publicly reported studies on optical materials composed of PMN-PT related crystals and glass. In 1998, Lee et al. disclosed 30PbO-30TiO 2 -(40–x)B 2 O 3 -xBaO (0 < x < 20 mol%) glass (Lee S W, Shim K B, Auh K H, et al. Ferroelectric anomaly in the differential thermal analysis of PbTiO 3 glass [J]. Materials Letters, 1999, 38: 356-359), and precipitated PbTiO 3Ferroelectric crystals, through DTA differential thermal analysis, the ferroelectric anomaly of its composite materials was discovered, that is, the phase change endothermic peak near the Curie temperature, and the Curie temperature decreases with the increase of BaO content; in 2020, Yang Zhongmin et al. invented ferroelectric microcrystalline glass (Yang Zhongmin, Shi Zhenguo, Zhou Shifeng, A Ferroelectric Property Continuous and Tunable Bi 2 GeO 5 Ferroelectric Microcrystalline Glass and Its Preparation Method [P], Chinese Invention, 2020, CN 111533457A), using heat treatment crystallization technology, prepared ferroelectric glass with Bi 2 GeO 5 microcrystals; however, when using this heat treatment crystallization technology to prepare ferroelectric microcrystalline glass, the crystals mainly precipitate on the surface, and the crystallinity is low, making it difficult to control and realize the batch preparation of ferroelectric microcrystalline glass with high crystallinity and full homogeneity. Summary of the Invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a ferroelectric micro-nano crystal glass, its preparation and application, which fully utilizes the advantages of high-performance ferroelectric crystals and high-transparency glass, not only meets the adjustable crystallinity and size of the ferroelectric crystal phase, but also has a simple and easy preparation method.

[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A ferroelectric micro-nano crystal glass, the matrix glass material is 70TeO 2 -(10+x)ZnO-(20-x)Na 2 O(0<x<10) tellurite glass, the doped crystal material is (1-y)Pb(Mg 1 / 3 Nb 2 / 3 )O 3 -yPbTiO 3 (0.4<y<0.2) compound crystal, and the content of the doped compound crystal is 0.1wt%-50wt%.

[0007] A preparation method of a ferroelectric micro-nano crystal glass, comprising the following steps:

[0008] 1) Mixing tellurite glass and PMN-PT crystals: Weigh tellurium oxide powder (5N), zinc oxide powder (5N) and sodium carbonate powder (5N) in proportion, and mix them evenly for use as glass raw materials; use a planetary high-speed ball mill to mill PMN-PT crystals, and after drying, sieving and testing with a laser particle size analyzer, obtain crystal powder with D90 in the micron range, that is, 90% of the powder particle size is less than the micron range, for use as doped crystals;

[0009] 2) One-step melting of microcrystalline glass: Put the glass raw materials into a crucible, place it in a muffle furnace, melt it at a temperature of 700-900℃, melt it for more than half an hour, and then cool it to 550-600℃; dope the doped crystals into the glass melt, stir it and then discharge it, pour it into a mold for annealing, and obtain ferroelectric micro-nanocrystalline glass.

[0010] An application of ferroelectric micro-nano crystal glass. Ferroelectric micro-nano crystal glass with a small amount of 0.1-10% doped crystal can be used for nonlinear optics; ferroelectric micro-nano crystal glass with a large amount of 10-50% doped crystal can be used as dielectric material.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] (1) The present invention combines the advantages of tellurite glass and PMN-PT crystal to prepare a composite material ferroelectric micro-nanocrystalline glass by melting in one step, which is easy to prepare in batches. The selection of materials can meet the requirements for efficient preparation of this ferroelectric micro-nanocrystalline glass. The tellurite glass used as the matrix material has a glass softening temperature T s The melting point of PMN-PT crystals is about 400℃, and the melting point of PMN-PT crystals as doped crystal materials is about 1400℃. When ferroelectric micro-nanocrystalline glass is melted at a high temperature of about 700℃-900℃, the glass raw materials melt to generate tellurite glass, and the temperature is lowered to about 550℃-600℃ for doping crystals and stirring to discharge, which effectively avoids PMN-PT crystals from being thermally etched, and is easy to control the crystal size and concentration to achieve high crystallinity and full homogeneity.

[0013] (2) The ferroelectric micro-nanocrystalline glass of the present invention, by virtue of the similar refractive index of tellurite matrix glass and PMN-PT ferroelectric crystal, is melted in one step to obtain PMN-PT nanocrystal doped glass with good light transmittance. The appropriate amount of doping can still have a high transmittance of more than 60% in the 500-5000nm optical band, and can also have high nonlinear optical performance.

[0014] (3) The heavily doped ferroelectric micro-nanocrystalline glass of the present invention can have both the electrical breakdown resistance of glass and the dielectric energy storage of ferroelectric crystals. By optimizing the mass fraction or volume fraction ratio, dielectric materials with high electrical breakdown strength and high energy storage density can be further prepared. The present invention provides a new method for new ferroelectric microcrystalline glass, and provides an ideal basic material for manufacturing ferroelectric functional energy storage capacitors and microwave dielectrics, and even optical modulators. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a flow chart of the preparation method of the embodiment of the present invention.

[0016] Figure 2 This is the actual image and XRD spectrum of the ferroelectric micro-nanocrystalline glass in Example 1 of the present invention.

[0017] Figure 3 This is the transmission spectrum of the ferroelectric micro-nanocrystalline glass in Example 1 of the present invention. DETAILED DESCRIPTION

[0018] In order to better understand the present invention, the contents of the present invention are further explained below in conjunction with examples, but the embodiments of the present invention are not limited thereto, and the process parameters not particularly described can be carried out with reference to conventional techniques.

[0019] Example 1: A ferroelectric micro-nanocrystalline glass, wherein the matrix glass material is 70TeO 2 -10ZnO-20Na 2 O tellurite glass, doped with 0.72Pb(Mg 1 / 3 Nb 2 / 3 ) 3 -0.28PbTiO 3 The compound crystal has a doped compound crystal content of 0.5wt%.

[0020] like Figure 1 As shown, a method for preparing ferroelectric micro-nanocrystalline glass comprises the following steps:

[0021] 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder (5N), zinc oxide powder (5N) and sodium carbonate powder (5N) are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball milling, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e., 90% of the powder particle size is less than micron level, which is reserved as doping crystals;

[0022] In this embodiment, the glass raw material is 70TeO 2 -10ZnO-20Na 2 The formula of O is:

[0023] TeO 2 : 70 mol%;

[0024] ZnO: 10 mol%;

[0025] Na 2 O: 20 mol%

[0026] In terms of molar percentage, the formula of doped crystal 72PMN-28PT is:

[0027] Pb(Mg 1 / 3 Nb 2 / 3 ) 3 :72mol%;

[0028] PbTiO 3:28mol%;

[0029] 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, tellurite glass is pre-melted at 750°C, melted for more than half an hour, and cooled to 550 degrees; doped crystals are doped into the glass melt at a mass percentage of 0.5wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

[0030] The physical picture of the ferroelectric micro-nanocrystalline glass and the XRD spectrum of the glass powder in this embodiment are as follows: Figure 2 As shown, there is no obvious crystal peak when PMN-PT is doped within 5%, and an obvious PMN-PT crystal peak appears when the doping is 5-20%. The transmittance spectrum of ferroelectric micro-nanocrystalline glass is shown in Figure 3 As shown, it can be seen that the transmittance of undoped glass in the 0.5-2μm band is nearly 80%, while it is close to 70% after doping with 0.5% PMN-PT crystal. The inset is the spectrum after 1.064μm laser enters the doped nanocrystal glass, showing 0.532μm doubled frequency light and residual 1.064μm light. This ferroelectric micro-nanocrystalline glass can be used for high transparency and high nonlinear glass optical fiber drawing applications.

[0031] Beneficial effects of this embodiment: The XRD crystal phase spectrum of the ferroelectric micro-nanocrystalline glass is as follows: Figure 2 As shown in Figure 2, it shows that the PMN-PT ferroelectric crystal is well preserved in the one-step melting process; the transmittance spectrum of the ferroelectric micro-nanocrystalline glass is shown in Figure 2. Figure 3 As shown, it is proved that the microcrystalline glass with 0.5% PMN-PT doped crystals still has a high transmittance; the ferroelectric micro-nanocrystalline glass can be used for high-transparency and high-nonlinear glass optical fiber drawing applications, and the highly doped microcrystalline glass is also expected to be used in dielectric materials.

[0032] Example 2, a ferroelectric micro-nanocrystalline glass, the matrix glass material is 70TeO 2 -15ZnO-15Na 2 O tellurite glass, doped with 0.6Pb(Mg 1 / 3 Nb 2 / 3 ) 3 -0.4PbTiO 3 The compound crystal has a doped compound crystal content of 0.1 wt%.

[0033] A method for preparing ferroelectric micro-nanocrystalline glass comprises the following steps:

[0034] 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder (5N), zinc oxide powder (5N) and sodium carbonate powder (5N) are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball milling, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e., 90% of the powder particle size is less than micron level, which is reserved as doping crystals;

[0035] In this embodiment, the glass raw material is 70TeO 2 -15ZnO-15Na 2 The formula of O is:

[0036] TeO 2 : 70 mol%;

[0037] ZnO: 15 mol%;

[0038] Na 2 O: 15 mol%

[0039] In terms of molar percentage, the formula of doped crystal 60PMN-40PT is:

[0040] Pb(Mg 1 / 3 Nb 2 / 3 ) 3 :60mol%;

[0041] PbTiO 3 :40mol%;

[0042] 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, tellurite glass is pre-melted at 900°C, melted for more than half an hour, and cooled to 580 degrees; doped crystals are doped into the glass melt at a mass percentage of 0.1wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

[0043] The physical picture of the ferroelectric micro-nanocrystalline glass, the XRD spectrum of the glass powder and the application of this embodiment are similar to those of embodiment 1.

[0044] Example 3, a ferroelectric micro-nanocrystalline glass, the matrix glass material is 70TeO 2 -15ZnO-15Na 2 O tellurite glass, doped with 0.8Pb(Mg 1 / 3 Nb 2 / 3 ) 3 -0.2PbTiO 3 The compound crystal has a doped compound crystal content of 50 wt%.

[0045] A method for preparing ferroelectric micro-nanocrystalline glass comprises the following steps:

[0046] 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder (5N), zinc oxide powder (5N) and sodium carbonate powder (5N) are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball milling, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e., 90% of the powder particle size is less than micron level, which is reserved as doping crystals;

[0047] In this embodiment, the glass raw material is 70TeO 2 -15ZnO-15Na 2 The formula of O is:

[0048] TeO 2 : 70 mol%;

[0049] ZnO: 15 mol%;

[0050] Na 2 O: 15 mol%

[0051] In terms of molar percentage, the formula of doped crystal 80PMN-20PT is:

[0052] Pb(Mg 1 / 3 Nb 2 / 3 ) 3 :80mol%;

[0053] PbTiO 3 :20mol%;

[0054] 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, tellurite glass is pre-melted at 700°C, melted for more than half an hour, and cooled to 600 degrees; doped crystals are doped into the glass melt at a mass percentage of 50wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

[0055] The actual ferroelectric micro-nanocrystalline glass of this embodiment is opaque and can be used for dielectric materials, such as capacitors with high resistance to breakdown.

Claims

1. A ferroelectric micro-nanocrystalline glass, characterized in that: The matrix glass material is 70TeO2-(10+x)ZnO-(20-x)Na2O tellurite glass, where 0<x<10, and the doped crystal material is (1-y)Pb(Mg 1 / 3 Nb 2 / 3 )O3-yPbTiO3 compound crystal, where 0.4<y<0.2, and the content of the doped compound crystal is 0.1 - 50 wt%.

2. The method for preparing ferroelectric micro-nanocrystalline glass according to claim 1, characterized in that: The following steps are involved: 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder, zinc oxide powder and sodium carbonate powder are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball mill, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e. 90% of the powder particle size is less than micron level, which is reserved as doped crystals; 2) One-step melting of microcrystalline glass: Put the glass raw materials into a crucible, place it in a muffle furnace, melt it at a temperature of 700-900℃, melt it for more than half an hour, and then cool it down to 550-600℃; dope the doped crystals into the glass melt, stir it and then discharge it, pour it into a mold for annealing, and obtain ferroelectric micro-nanocrystalline glass.

3. A ferroelectric micro-nanocrystalline glass, characterized in that: The matrix glass material is 70TeO2-10ZnO-20Na2O tellurite glass, and the doped crystal material is 0.72Pb(Mg 1 / 3 Nb 2 / 3 5 wt% )O3-0.28PbTiO3 compound crystals, the doped compound crystal content is 0.5 wt%.

4. The method for preparing ferroelectric micro-nanocrystalline glass according to claim 3, characterized in that: The following steps are involved: 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder, zinc oxide powder and sodium carbonate powder are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball mill, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e. 90% of the powder particle size is less than micron level, which is reserved as doped crystals; In terms of molar percentage, the formula of glass raw material 70TeO2-10ZnO-20Na2O is: TeO2: 70 mol% ZnO: 10 mol %; Na2O: 20 mol% In terms of molar percentage, the formula of doped crystal 72PMN-28PT is: Pb(Mg 1 / 3 Nb 2 / 3 )O3: 72 mol %; PbTiO3: 28 mol %; 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, and tellurite glass is pre-melted at 750°C for more than half an hour, and then cooled to 550°C; doped crystals are doped into the glass melt at a mass percentage of 0.5 wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

5. A ferroelectric micro-nanocrystalline glass, characterized in that: The matrix glass material is 70TeO2-15ZnO-15Na2O tellurite glass, and the doped crystal material is 0.6Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.4PbTiO3 compound crystals, the doped compound crystal content is 0.1 wt%.

6. The method for preparing ferroelectric micro-nanocrystalline glass according to claim 5, characterized in that: The following steps are involved: 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder, zinc oxide powder and sodium carbonate powder are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball mill, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e. 90% of the powder particle size is less than micron level, which is reserved as doped crystals; In terms of molar percentage, the formula of glass raw material 70TeO2-15ZnO-15Na2O is: TeO2: 70 mol% ZnO: 15mol%; Na2O: 15 mol% In terms of molar percentage, the formula of doped crystal 60PMN-40PT is: Pb(Mg 1 / 3 Nb 2 / 3 )O3: 60 mol %; PbTiO3: 40mol %; 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, tellurite glass is pre-melted at 900°C, melted for more than half an hour, and then cooled to 580°C; doped crystals are doped into the glass melt at a mass percentage of 0.1 wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

7. A ferroelectric micro-nanocrystalline glass, characterized in that: The matrix glass material is 70TeO2-15ZnO-15Na2O tellurite glass, and the doped crystal material is 0.8Pb(Mg 1 / 3 Nb 2 / 3 )O3-0.2PbTiO3 compound crystals, the doped compound crystal content is 50 wt%.

8. The method for preparing ferroelectric micro-nanocrystalline glass according to claim 7, characterized in that: The following steps are involved: 1) Tellurite glass and PMN-PT crystal mixing: Tellurium oxide powder, zinc oxide powder and sodium carbonate powder are prepared in proportion, mixed evenly and reserved as glass raw materials; PMN-PT crystals are milled by planetary high-speed ball mill, dried, sieved and tested by laser particle size analyzer to obtain crystal powder with D90 of micron level, i.e. 90% of the powder particle size is less than micron level, which is reserved as doped crystals; In terms of molar percentage, the formula of glass raw material 70TeO2-15ZnO-15Na2O is: TeO2: 70 mol% ZnO: 15 mol %; Na2O: 15 mol% In terms of molar percentage, the formula of doped crystal 80PMN-20PT is: Pb(Mg 1 / 3 Nb 2 / 3 )O3: 80mol %; PbTiO3: 20 mol %; 2) One-step melting of microcrystalline glass: glass raw materials are loaded into an alumina crucible, placed in a muffle furnace, and tellurite glass is pre-melted at 700°C for more than half an hour, and then cooled to 600°C; doped crystals are doped into the glass melt at a mass percentage of 50wt%, stirred for 1 minute, and then discharged, poured into a mold at 320°C, annealed for 3 hours, and then slowly cooled to room temperature to obtain uniform ferroelectric micro-nanocrystalline glass.

9. The use of a ferroelectric micro-nanocrystalline glass according to claim 1, 3, 5 or 7, characterized in that: Ferroelectric micro-nanocrystalline glass with a small amount of 0.1-10% doped crystals is used for nonlinear optics; ferroelectric micro-nanocrystalline glass with a small amount of 10-50% doped crystals is used for dielectric materials.