A carburizing and quenching strengthening process for 20CrMo cylinder body for hydraulic breaker

Through vacuum carburizing and quenching technology, the carburizing pulse and vacuum air quenching treatment are used to solve the problems of low carburizing efficiency and serious internal oxidation in traditional atmosphere carburizing treatment, and the surface hardness and core hardness of the cylinder in 20CrMo are improved. Extend service life.

CN117418187BActive Publication Date: 2024-11-12XUZHOU BUT CONSTR MASCH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311517895.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-11-12
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

The traditional atmosphere carburizing treatment process leads to low carburizing efficiency of the cylinder in 20CrMo, uneven depth of the carburizing layer, and severe internal oxidation, which affects its service life.

Method used

The vacuum carburizing and quenching process is adopted, including pre-oxidation treatment, vacuum carburizing treatment, quenching treatment and low-temperature tempering treatment. Carburizing efficiency is improved through carburizing pulse mode and vacuum air quenching to avoid internal oxidation.

Benefits of technology

It improves carburizing efficiency, improves the problems of uneven depth of carburizing layer and oxidation within the surface, and improves product quality and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117418187B_ABST
    Figure CN117418187B_ABST
Patent Text Reader

Abstract

The invention discloses a carburizing and quenching strengthening process for a 20CrMo cylinder body for a hydraulic breaker, comprising the following steps: step 1, pre-oxidation treatment, placing the 20CrMo cylinder body for a hydraulic breaker in a preheating furnace, heating, heat preservation, and then taking it out of the furnace; step 2, vacuum carburizing treatment, placing the cylinder body in a vacuum carburizing furnace, evacuating, and carburizing by a carburizing pulse method; step 3, quenching treatment, introducing nitrogen after carburizing, rapidly cooling, heat preservation, and vacuum gas quenching; step 4, low-temperature tempering treatment, placing the cylinder body in a tempering furnace, heat preservation, and then air cooling. The invention improves the carburizing efficiency, improves the problems of uneven carburizing layer depth and surface internal oxidation, improves product quality, and shortens the production cycle by performing vacuum low-pressure carburizing and quenching treatment on the 20CrMo cylinder body, and meets the performance indicators such as the thickness of the carburized layer, the surface hardness, and the core hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment of low-carbon alloy structural steel, in particular to a carburizing and quenching strengthening process for a 20CrMo cylinder body used for a hydraulic breaker. Background Art

[0002] The complex service conditions and failure forms of the cylinder of the hydraulic breaker require that the surface of the cylinder should have high hardness and high wear resistance, and the core should have good plasticity and toughness. At present, the materials commonly used to manufacture the cylinder of the hydraulic breaker at home and abroad are mainly low-carbon alloy steels, such as 20CrMo steel. Its surface hardness after carburizing can reach more than HRC58, and it has excellent wear resistance. At the same time, its core has good strength and toughness after quenching, and has good comprehensive mechanical properties. Therefore, the heat treatment process is a key factor affecting the quality of the cylinder product. The commonly used heat treatment processes of 20CrMo mainly include atmosphere carburizing, quenching, low-temperature tempering and other processes. However, the traditional atmosphere carburizing treatment process has problems such as low carburizing efficiency, uneven carburizing layer depth, and severe internal oxidation, which reduces the service performance of the 20CrMo cylinder. Therefore, it is necessary to improve the carburizing and quenching strengthening process of the 20CrMo cylinder for hydraulic breaker to increase its service life. Summary of the invention

[0003] The purpose of the present invention is to provide a carburizing and quenching strengthening process for a 20CrMo cylinder body for a hydraulic breaker, so as to solve the problems of low carburizing efficiency, uneven carburizing layer depth and severe internal oxidation of a 20CrMo cylinder body for a hydraulic breaker in the prior art.

[0004] To achieve the above object, the present invention adopts the following technical solution:

[0005] A carburizing and quenching strengthening process for a 20CrMo cylinder body for a hydraulic breaker comprises the following steps:

[0006] Step 1, pre-oxidation treatment, placing the 20CrMo cylinder body of the hydraulic breaker in a preheating furnace, heating, keeping warm, and then taking it out of the furnace;

[0007] Step 2, vacuum carburizing treatment, placing the middle cylinder body in a vacuum carburizing furnace, evacuating the vacuum, and carburizing by carburizing pulse method;

[0008] Step 3, quenching treatment, after carburizing, nitrogen is introduced to quickly cool down, and after heat preservation, vacuum quenching is performed;

[0009] Step 4, low temperature tempering treatment, placing the middle cylinder body in a tempering furnace, keeping warm, and then air cooling.

[0010] Furthermore, in step 1, heating is performed in an air atmosphere at a heating temperature of 500° C. and a heat preservation time of 60 minutes.

[0011] Furthermore, in step 2, the furnace is evacuated to a pressure less than 10 Pa, heated to 650° C., kept warm for 60 minutes, and then heated to 930-980° C. before carburizing.

[0012] Furthermore, in the step 2, when carburizing is performed by carburizing pulse method, a pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse. That is, in the strong carburizing pulse stage, carburizing atmosphere is filled into the furnace, and the pressure is stabilized at 300Pa for 2 minutes. In the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable 70Pa for (0.7-2.8)*n minutes, where n is the nth pulse. After that, the gas is quickly evacuated and filled with carburizing atmosphere to execute the next carburizing pulse. The total number of pulses is 16-41 times.

[0013] Furthermore, in step 2, the carburizing atmosphere is high-purity acetylene.

[0014] Furthermore, in the step 3, the temperature is rapidly lowered to a quenching temperature of 830° C., kept at that temperature for 60 minutes, and then vacuum quenched.

[0015] Furthermore, in step 3, the atmosphere used for vacuum quenching is a mixed gas of helium and nitrogen with a pressure of 15 bar.

[0016] Furthermore, in step 4, the middle cylinder body is placed in a tempering furnace at a temperature of 190° C. for 8 hours.

[0017] Furthermore, the chemical composition of the material of the 20CrMo cylinder body meets the requirements of GB / T3077-2015 standard; the smelting method of the material of the 20CrMo cylinder body is electric furnace smelting, the forging adopts free forging, the forging ratio is ≥3, and the 880-920℃ normalizing is adopted.

[0018] Beneficial effect: The carburizing and quenching strengthening process of the 20CrMo cylinder body for hydraulic breaker provided by the present invention is not only applicable to the carburizing and quenching 20CrMo cylinder body for hydraulic breaker, but also applicable to all other workpieces of 20CrMo material that need to be carburized and quenched. The carburizing and quenching strengthening process of the 20CrMo cylinder body for hydraulic breaker provided by the present invention adopts a vacuum carburizing and quenching process to replace the traditional atmosphere carburizing and quenching. On the premise of meeting the performance indicators such as surface hardness, thickness of carburized layer, and core hardness, the carburizing efficiency is improved, the uneven depth of carburized layer and the internal oxidation of the surface are improved, the product quality is improved, and the production cycle is shortened. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of hardness test sampling points;

[0020] Figure 2This is a surface metallographic photograph of the 20CrMo cylinder body obtained in Example 1;

[0021] Figure 3 This is a metallographic photograph of the core of the 20CrMo cylinder body obtained in Example 1;

[0022] Figure 4 This is a photo of the depth of the oxide layer on the surface of the 20CrMo cylinder body obtained in Example 1;

[0023] Figure 5 This is a surface metallographic photograph of the 20CrMo cylinder body obtained in Example 2;

[0024] Figure 6 This is a metallographic photograph of the core of the 20CrMo cylinder body obtained in Example 2;

[0025] Figure 7 This is a photo of the depth of the oxide layer on the surface of the 20CrMo cylinder body obtained in Example 2;

[0026] Figure 8 This is a surface metallographic photograph of the 20CrMo cylinder body obtained in Example 3;

[0027] Fig. 9 This is a metallographic photograph of the core of the 20CrMo cylinder body obtained in Example 3;

[0028] Fig.10 This is a photo of the depth of the oxide layer on the surface of the 20CrMo cylinder body obtained in Example 3;

[0029] Fig.11 This is a metallographic photograph of the surface of the 20CrMo cylinder body obtained in the comparative example;

[0030] Fig.12 This is a metallographic photograph of the core of the 20CrMo cylinder body obtained in the comparative example;

[0031] Fig.13 This is a photo of the depth of the oxide layer on the surface of the 20CrMo cylinder block obtained in the comparative example. DETAILED DESCRIPTION

[0032] The present invention provides a carburizing and quenching strengthening process for a 20CrMo cylinder body for a hydraulic breaker. The chemical composition of the material of the 20CrMo cylinder body meets the requirements of the GB / T3077-2015 standard. The smelting method of the material of the 20CrMo cylinder body is electric furnace smelting, the forging adopts free forging, the forging ratio is ≥3, and the 880-920℃ normalizing is performed. The process comprises the following steps:

[0033] (1) Pre-oxidation treatment: the middle cylinder is placed in a preheating furnace and heated in an air atmosphere at a heating temperature of 500°C for a holding time of 60 minutes, and then taken out of the furnace;

[0034] (2) Vacuum carburizing treatment, placing the middle cylinder in a vacuum carburizing furnace, evacuating the furnace until the pressure inside is less than 10Pa, heating to 650°C, keeping the temperature for 60 minutes, further heating to 930-980°C, and carburizing by pulse carburizing. One pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse. That is, in the strong carburizing pulse stage, high-purity acetylene is filled into the furnace, and the pressure is stabilized at 300Pa for 2 minutes. In the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable pressure of 70Pa for (0.7-2.8)*n minutes, where n is the nth pulse. Then, the gas is quickly evacuated and filled with carburizing atmosphere to execute the next carburizing pulse. The total number of pulses is 16-41 times.

[0035] (3) Quenching treatment: after carburizing, nitrogen is introduced to rapidly cool the temperature to 830°C, and after keeping the temperature for 60 min, vacuum quenching is performed. The atmosphere used for vacuum quenching is a mixture of helium and nitrogen at a pressure of 15 bar.

[0036] (4) Low-temperature tempering treatment: place the middle cylinder body in a tempering furnace at a temperature of 190°C for 8 hours, and then air cool.

[0037] The carburizing and quenching strengthening process of the 20CrMo cylinder body for the hydraulic breaker provided by the present invention is described in detail below in conjunction with the embodiments.

[0038] Example 1

[0039] The 20CrMo cylinder material for the breaker has the following chemical compositions: C: 0.226wt.%; Mn: 0.593wt.%; Si: 0.266wt.%; P: 0.014wt.%; S: 0.004wt.%; Cr: 0.987wt.%; Mo: 0.175wt.%. The 20CrMo cylinder is carburized and quenched to strengthen the treatment, including the following steps:

[0040] (1) Pre-oxidation treatment: the middle cylinder is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0041] (2) Vacuum carburizing treatment, placing the middle cylinder in a vacuum carburizing furnace, evacuating the furnace until the pressure inside is less than 10Pa, heating to 650°C, keeping the temperature for 60 minutes, further heating to 930°C, and carburizing by pulse carburizing. One pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse. That is, in the strong carburizing pulse stage, high-purity acetylene is filled into the furnace, and the pressure is stabilized at 300Pa for 2 minutes. In the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable pressure of 70Pa for 0.7*n minutes, where n is the nth pulse. Then, the gas is quickly evacuated and filled with carburizing atmosphere to execute the next carburizing pulse. The total number of pulses is 41 times.

[0042] (3) Quenching treatment: after carburizing, nitrogen is introduced to rapidly cool the temperature to 830°C, and after keeping the temperature for 60 min, vacuum quenching is performed. The atmosphere used for vacuum quenching is a mixture of helium and nitrogen at a pressure of 15 bar.

[0043] (4) Low-temperature tempering treatment: place the middle cylinder body in a tempering furnace at a temperature of 190°C for 8 hours, and then air cool.

[0044] The performance indicators of the 20CrMo cylinder block obtained after carburizing and quenching heat treatment in Example 1 were tested. The performance test results are shown in Table 1, and the metallographic photos of the surface, the core and the internal oxidation are shown in Table 1. Figure 2 , Figure 3 , Figure 4 As shown. It can be seen that the surface metallographic structure is needle-shaped martensite and a small amount of residual austenite, the core structure is lath martensite, there is no internal oxidation, the deepest carburized layer is 1.71mm, the shallowest is 1.57mm, and the depth difference is 0.14mm.

[0045] Table 1 Performance index of Example 1

[0046]

[0047] Example 2

[0048] The 20CrMo cylinder material for the breaker has the following chemical compositions: C: 0.226wt.%; Mn: 0.593wt.%; Si: 0.266wt.%; P: 0.014wt.%; S: 0.004wt.%; Cr: 0.987wt.%; Mo: 0.175wt.%. The 20CrMo cylinder is carburized and quenched to strengthen the treatment, including the following steps:

[0049] (1) Pre-oxidation treatment: the middle cylinder is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0050] (2) Vacuum carburizing treatment, placing the middle cylinder in a vacuum carburizing furnace, evacuating the furnace until the pressure inside is less than 10Pa, heating to 650°C, keeping the temperature for 60 minutes, further heating to 950°C, and carburizing by pulse carburizing. One pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse. That is, in the strong carburizing pulse stage, high-purity acetylene is filled into the furnace, and the pressure is stabilized at 300Pa for 2 minutes. In the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable pressure of 70Pa for 1.4*n minutes, where n is the nth pulse. Then, the gas is quickly evacuated and filled with carburizing atmosphere to execute the next carburizing pulse. The total number of pulses is 26 times.

[0051] (3) Quenching treatment: after carburizing, nitrogen is introduced to rapidly cool the temperature to 830°C, and after keeping the temperature for 60 min, vacuum quenching is performed. The atmosphere used for vacuum quenching is a mixture of helium and nitrogen at a pressure of 15 bar.

[0052] (4) Low-temperature tempering treatment: place the middle cylinder body in a tempering furnace at a temperature of 190°C for 8 hours, and then air cool.

[0053] The performance indicators of the 20CrMo cylinder block obtained after carburizing and quenching heat treatment in Example 2 were tested. The performance test results are shown in Table 2. The metallographic photos of the surface, the core and the internal oxidation are shown in Table 2. Figure 5 , Figure 6 , Figure 7 As shown. It can be seen that the surface metallographic structure is needle-shaped martensite and a small amount of residual austenite, the core structure is lath martensite, there is no internal oxidation, the deepest carburized layer is 1.72mm, the shallowest is 1.59mm, and the depth difference is 0.13mm.

[0054] Table 2 Performance index of Example 2

[0055]

[0056] Example 3

[0057] The 20CrMo cylinder material for the breaker has the following chemical compositions: C: 0.226wt.%; Mn: 0.593wt.%; Si: 0.266wt.%; P: 0.014wt.%; S: 0.004wt.%; Cr: 0.987wt.%; Mo: 0.175wt.%. The 20CrMo cylinder is carburized and quenched to strengthen the treatment, including the following steps:

[0058] (1) Pre-oxidation treatment: the middle cylinder is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0059] (2) Vacuum carburizing treatment, placing the middle cylinder in a vacuum carburizing furnace, evacuating the furnace until the pressure inside is less than 10Pa, heating to 650°C, keeping the temperature for 60 minutes, further heating to 980°C, and carburizing by pulse carburizing. One pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse. That is, in the strong carburizing pulse stage, high-purity acetylene is filled into the furnace, and the pressure is stabilized at 300Pa for 2 minutes. In the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable pressure of 70Pa for 2.8*n minutes, where n is the nth pulse. Then, the gas is quickly evacuated and filled with carburizing atmosphere to execute the next carburizing pulse. The total number of pulses is 16 times.

[0060] (3) Quenching treatment: after carburizing, nitrogen is introduced to rapidly cool the temperature to 830°C, and after keeping the temperature for 60 min, vacuum quenching is performed. The atmosphere used for vacuum quenching is a mixture of helium and nitrogen at a pressure of 15 bar.

[0061] (4) Low-temperature tempering treatment: place the middle cylinder body in a tempering furnace at a temperature of 190°C for 8 hours, and then air cool.

[0062] The performance indicators of the 20CrMo cylinder block obtained after carburizing and quenching heat treatment in Example 3 were tested. The performance test results are shown in Table 3. The metallographic photos of the surface, the core and the internal oxidation are shown in Table 3. Figure 8 , Fig. 9 , Fig.10 As shown. It can be seen that the surface metallographic structure is needle-shaped martensite and a small amount of residual austenite, the core structure is lath martensite, there is no internal oxidation, the deepest carburized layer is 1.69mm, the shallowest is 1.58mm, and the depth difference is 0.11mm.

[0063] Table 3 Performance index of Example 3

[0064]

[0065] Comparative Example

[0066] The 20CrMo cylinder material for the breaker has the following chemical compositions: C: 0.226wt.%; Mn: 0.593wt.%; Si: 0.266wt.%; P: 0.014wt.%; S: 0.004wt.%; Cr: 0.987wt.%; Mo: 0.175wt.%. The 20CrMo cylinder is carburized and quenched to strengthen the treatment, including the following steps:

[0067] (1) Pre-oxidation treatment: the middle cylinder is placed in a preheating furnace and heated in an air atmosphere at a temperature of 500°C for 60 minutes, and then taken out of the furnace for carburizing;

[0068] (2) Carburizing treatment, including three stages: heating, strong carburizing and diffusion. The carburizing atmosphere is nitrogen, methanol and propane. The heating stage is 850°C for 60 minutes after the middle cylinder enters the carburizing furnace. The carbon potential in the heating stage is 0.6%. The temperature of the strong carburizing and diffusion stages is 930°C. The holding time in the strong carburizing stage is 600 minutes, and the carbon potential is 1.2%. The holding time in the diffusion stage is 540 minutes, and the carbon potential is 0.85%;

[0069] (4) Quenching treatment: first keep the temperature at 830°C for 60 minutes, the carbon potential is 0.8%, then immerse in quenching oil for cooling, the quenching oil temperature is 60°C, keep the temperature in the quenching oil for 60 minutes, and the stirring frequency of the quenching oil is 30 Hz;

[0070] (6) Low-temperature tempering treatment: place the middle cylinder body in a tempering furnace at a temperature of 190°C for 480 minutes, and then air-cool to room temperature.

[0071] The performance indexes of the 20CrMo cylinder block obtained after carburizing and quenching heat treatment in the comparative example were tested. The performance test results are shown in Table 4. The metallographic photos of the surface, the core and the internal oxidation are shown in Table 4. Fig.11 , Fig.12 , Fig.13 It can be seen that the surface metallographic structure is needle-shaped martensite and a small amount of residual austenite, the core structure is lath martensite, the inner oxide layer depth exceeds 20μm, the inner oxide layer depth and carburizing time are much higher than those in the embodiment, the deepest carburizing layer is 1.84mm and the shallowest is 1.40mm, the depth difference is 0.44mm, and the depth difference of the carburizing layer is also much greater than that in the embodiment.

[0072] Table 4 Comparative Examples Performance Index

[0073]

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A carburizing and quenching strengthening process for a 20CrMo cylinder body for a hydraulic breaker, characterized in that: The following steps are involved: Step 1, pre-oxidation treatment, placing the 20CrMo cylinder body of the hydraulic breaker in a preheating furnace, heating it in an air atmosphere at a heating temperature of 500°C for 60 minutes, and then taking it out of the furnace; Step 2, vacuum carburizing treatment, placing the middle cylinder body in a vacuum carburizing furnace, evacuating the furnace until the pressure in the furnace is less than 10 Pa, heating to 650°C, keeping warm for 60 minutes, and then heating to 930-980°C, and then carburizing by carburizing pulse mode; when carburizing by carburizing pulse mode, a pulse carburizing includes two stages: strong carburizing pulse and diffusion pulse, that is, in the strong carburizing pulse stage, the furnace is filled with carburizing atmosphere, the pressure is stabilized at 300 Pa, the time is 2 minutes, in the diffusion pulse stage, the gas in the furnace is quickly evacuated and filled with nitrogen, and the pressure is adjusted to a stable pressure of 70Pa, the time is (0.7-2.8)*n minutes, n is the nth pulse, and then the gas is quickly evacuated and filled with carburizing atmosphere, and the next carburizing pulse is executed, and the total number of pulses is 16-41 times; Step 3, quenching treatment, after carburizing, nitrogen is introduced, the temperature is quickly lowered to the quenching temperature of 830°C, and after keeping the temperature for 60 minutes, vacuum quenching is performed. The atmosphere used for vacuum quenching is a mixed gas of helium and nitrogen with a pressure of 15 bar; Step 4, low temperature tempering treatment, placing the middle cylinder body in a tempering furnace at a temperature of 190°C, keeping warm for 8 hours, and then air cooling.

2. The carburizing and quenching strengthening process of a 20CrMo cylinder body for a hydraulic breaker according to claim 1 is characterized in that: In step 2, the carburizing atmosphere is high-purity acetylene.

3. The carburizing and quenching strengthening process of the 20CrMo cylinder body for a hydraulic breaker according to claim 1 is characterized in that: The chemical composition of the material of the 20CrMo cylinder body meets the requirements of GB / T3077-2015 standard; the smelting method of the material of the 20CrMo cylinder body is electric furnace smelting, the forging adopts free forging, the forging ratio is ≥3, and the 880-920℃ normalizing is adopted.