Hot pressing shaping method for ceramic reinforced aluminum matrix composite brake disc body
By adjusting the content of low-melting point alloy elements in the brake disc body of the ceramic-reinforced aluminum-based composite material and the hot pressing shaping method, the problem of taking into account the temperature resistance and structural strength of the brake disc body of the ceramic-reinforced aluminum-based composite material is solved. It achieves both temperature resistance and strength, and avoids interface cracking and meets braking requirements.
Patent Information
- Application Number
- CN202311448081.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-11-02
AI Technical Summary
When the ceramic-reinforced aluminum-based composite brake disc body improves temperature resistance, it is difficult to take into account the structural strength. In traditional design, the difference in ceramic content leads to discontinuous thermal expansion coefficient gradients, which is prone to interface cracking problems.
By adjusting the content of low-melting alloy elements in the brake disc body of the ceramic-reinforced aluminum-based composite material, the hot pressing shaping method is adopted to show a gradient decreasing pattern from the core to the outside, and a mold designed with a multi-ring area is used to achieve low The uniform distribution and flow control of melting point alloy elements ensure the temperature resistance and core strength of the disk surface.
The temperature resistance and structural strength of the ceramic-reinforced aluminum-based composite brake disc body are achieved, which avoids interface cracking, meets the braking requirements of the brake disc, and improves durability during use.
Smart Images

Figure CN117444206B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder metallurgy, in particular to a hot pressing shaping method for a brake disc body of a ceramic reinforced aluminum-based composite material. Background Art
[0002] The brake disc is a friction pair of the disc brake. The friction between the disc surface and the brake pad generates a lot of heat, which requires the disc surface to withstand a high temperature. Otherwise, it is easy to soften at high temperature, resulting in a sharp drop in the friction coefficient and abnormal wear, which will cause the brake disc to fail. The ceramic reinforced aluminum-based composite brake disc body generally improves the temperature resistance by increasing the ceramic particle content, but as the ceramic particle content increases, it is bound to affect the bonding between the reinforcement phase and the matrix, thereby affecting the mechanical properties of the disc body. Therefore, it is urgent to solve the problem that the temperature resistance and structural strength of the ceramic reinforced aluminum-based composite brake disc body cannot be taken into account.
[0003] Traditional solutions mostly use a "sandwich" structure of ceramic-reinforced aluminum-based composite brake disc body, that is, a design mode with high ceramic content on the outside and low ceramic content in the core. However, due to the large difference in ceramic content, the thermal expansion coefficient between the two materials is also very different, which is prone to gradient discontinuity, difficulty in combining interfaces during the production process, and interface cracking after multiple hot and cold shocks during use.
[0004] After extensive research, the inventor of this application found that by adjusting the content of alloy elements that can form low-melting-point eutectic components (referred to as low-melting-point alloy elements in this application) in the disc body of a ceramic-reinforced aluminum-based composite brake disc, the content of low-melting-point alloy elements from the core to the outside of the disc body presents a gradient decreasing pattern, which can make the disc body surface have good temperature resistance while the core is high in strength and toughness, meeting the braking requirements of the brake disc. Therefore, how to achieve a gradient decrease in the content of low-melting-point alloy elements in the disc body from the core to the outside has become the focus of research. Summary of the invention
[0005] Based on this, it is necessary to provide a hot pressing shaping method for a ceramic reinforced aluminum-based composite brake disc body. This method can achieve a gradient decrease in the content of low-melting-point alloy elements in the disc body from the core to the outside, thereby ensuring both the temperature resistance of the disc body surface and the structural strength of the disc body, thereby meeting the braking requirements of the brake disc.
[0006] A hot pressing shaping method for a ceramic reinforced aluminum-based composite brake disc body comprises the following steps:
[0007] Providing a ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped;
[0008] A hot pressing shaping mold is provided, wherein the hot pressing shaping mold comprises an upper mold, a lower mold and a female mold. After the molds are closed, the upper mold and the lower mold are enclosed in the female mold to form a shaping cavity. The shaping cavity comprises a first part, a second part and a third part. The shape of the third part corresponds to the ceramic reinforced aluminum-based composite brake disc body to be hot pressed and shaped. The second part comprises a plurality of second annular areas symmetrically arranged on the upper and lower sides of the third part and equidistantly spaced in the radial direction. The first part comprises a plurality of first annular areas symmetrically arranged on the opposite sides of the second part and equidistantly spaced in the radial direction. The first annular areas on each side are respectively connected to the third part through the second annular areas on the respective sides.
[0009] The ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped is placed in the third part of the hot-pressing and shaped mold, and hot-pressing and shaped are performed after the mold is closed.
[0010] In one embodiment, the second annular zones on each side are equally spaced at a distance of 10 mm to 20 mm in the radial direction; the ring width of each second annular zone gradually decreases from the direction away from the third part to the direction close to the third part; the average ring width of each second annular zone is 5 um to 10 um; and the axial height of each second annular zone is 3 mm to 5 mm.
[0011] In one embodiment, the first annular areas on each side are equally spaced at a distance of 10 mm to 20 mm in the radial direction; the ring width of each first annular area gradually decreases from the direction away from the third part to the direction close to the third part; the average ring width of each first annular area is 3 mm to 5 mm; and the axial height of each first annular area is 3 mm to 5 mm.
[0012] In one embodiment, there are 4 to 8 first annular areas on each side.
[0013] In one embodiment, the ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped is prepared by the following method:
[0014] Provide ceramic reinforced aluminum matrix composite materials;
[0015] The ceramic reinforced aluminum-based composite material is pressed into shape and then sintered.
[0016] In one of the embodiments, the ceramic reinforced aluminum-based composite material consists of 40% to 60% ceramic particles and the remainder aluminum alloy, measured in mass percentage.
[0017] In one of the embodiments, the aluminum alloy consists of 1% to 4% copper, 1% to 4% magnesium and the balance aluminum, in terms of mass percentage.
[0018] In one embodiment, the temperature of the hot pressing shaping is between the solidus and liquidus of the aluminum alloy, and the pressure is 150 MPa to 300 MPa.
[0019] In one embodiment, the pressing pressure is 150 MPa to 300 MPa, and the holding time is 10 s to 30 s.
[0020] In one of the embodiments, the sintering temperature is 580° C. to 640° C., the time is 1 to 1.5 hours, and the heating rate is 5° C. / min to 10° C. / min.
[0021] The above-mentioned hot pressing shaping method of the ceramic reinforced aluminum-based composite brake disc body is as follows: the ceramic reinforced aluminum-based composite brake disc body to be hot pressed is placed in the third part of the hot pressing shaping mold, and hot pressing is performed after the mold is closed. The low-melting point alloy elements in the disc body form a liquid phase after reaching the eutectic point, and flow into the first annular area through the second annular areas on both sides. As the first annular area is gradually filled, the speed and amount of the liquid phase outflow will gradually decrease, thereby achieving a gradient structure in which the content of the low-melting point alloy elements in the disc body gradually decreases from the core to the outside, thereby ensuring both the temperature resistance of the disc surface and the structural strength of the disc body.
[0022] The brake disc prepared by the above method is not easy to crack during preparation and use, and can meet the braking requirements of the brake disc. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A three-dimensional cross-sectional view of a hot pressing and shaping mold in one embodiment;
[0024] Figure 2 for Figure 1 Schematic diagram of the mid-section. DETAILED DESCRIPTION
[0025] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below, and preferred embodiments of the present invention are provided. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0026] It should be noted that when an element is referred to as being "disposed" on another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0028] In addition, it should be noted that the “low melting point alloy element” in the present application refers to an alloy element that can form a low melting point eutectic component.
[0029] See also Figure 1 and 2 , is a hot pressing shaping mold of an embodiment, comprising an upper mold 12, a lower mold 14 and a female mold (not shown). After the molds are closed, the upper mold 12 and the lower mold 14 are enclosed in the female mold to form a shaping cavity (not shown).
[0030] The shaping cavity includes a first part 110 , a second part 120 and a third part 130 .
[0031] It can be understood that the shape of the third part 130 corresponds to the brake disc body to be shaped. In this embodiment, the brake disc body to be shaped is an annular blank, so the hot pressing shaping mold further includes a mandrel (not shown), the outer diameter of which matches the inner diameter of the annular blank.
[0032] The second part 120 includes a plurality of second annular areas 122 symmetrically arranged on the upper and lower sides of the third part 130 and spaced equidistantly in the radial direction. Further, the second annular areas 122 on each side are spaced equidistantly in the radial direction at a distance of 10 mm to 20 mm to ensure that the liquid phase will not be mixed or blocked during the flow process, thereby ensuring uniform distribution of the low-melting-point alloy element in the radial direction of the entire disk body.
[0033] Furthermore, the ring width of each second annular area 122 gradually decreases from a direction away from the third portion 130 to a direction close to the third portion 130 .
[0034] Furthermore, the average ring width of each second ring area 122 is 5 um to 10 um.
[0035] Furthermore, the axial height of each second annular area 122 is 3 mm to 5 mm.
[0036] The second annular region 122 is provided to ensure that the liquid phase can smoothly flow into the first annular region 112 without backflow.
[0037] The first part 110 includes a plurality of first annular areas 112 symmetrically arranged on opposite sides of the second part 120 and spaced equidistantly in the radial direction. The first annular areas 112 on each side are connected to the third part 130 through the second annular areas 122 on the respective sides. Further, the first annular areas 112 on each side are spaced equidistantly at a distance of 10 mm to 20 mm in the radial direction to ensure that the liquid phase flowing out of the corresponding position has enough space therein for diffusion and homogenization.
[0038] Furthermore, the ring width of each first annular area 112 gradually decreases from a direction away from the third portion 130 to a direction close to the third portion 130 .
[0039] Furthermore, the average ring width of each first annular area 112 is 3 mm to 5 mm.
[0040] Furthermore, the axial height of each first annular area 112 is 3 mm to 5 mm.
[0041] The first annular area 112 is provided to ensure that the liquid phase can flow smoothly and evenly fill the first annular area 112 without flowing back.
[0042] In this embodiment, there are 4 to 8 first annular areas 112 on each side. The second annular areas 122 correspond to the first annular areas 112 in position and are equal in number.
[0043] The ring width setting of the above-mentioned first annular area 112 and the second annular area 122 makes the ring width of the corresponding connected first annular area 112 and the second annular area 122 show a trend of gradually decreasing from the direction away from the third part 130 to the direction close to the third part 130 as a whole. Such a setting is conducive to a more uniform outflow of the liquid phase formed by the low-melting-point alloy element in the disk body, and as the first annular area 112 is gradually filled, the speed of the liquid phase outflow gradually slows down, thereby achieving a uniform decreasing trend of the content of the low-melting-point alloy element from the core to the outside of the disk body, further optimizing the performance of the disk body.
[0044] In addition, the ring width of the first annular zone 112 is significantly larger than the ring width of the second annular zone 122, which can not only control the flow speed and amount of the liquid phase, but also prevent the liquid phase from flowing back. This is because the ring width gradually decreases, and the liquid phase will encounter more and more resistance during the flow process, which prevents the liquid from flowing in the opposite direction, thereby ensuring that the content of low-melting-point alloy elements in the entire disk body presents a distribution trend that gradually decreases from the core to the outside, thereby ensuring that the surface of the disk body has good temperature resistance while the core has high strength and toughness.
[0045] The arrangement of the first annular area 112 and the second annular area 122 can ensure that the low-melting-point alloy elements flow out smoothly, thereby achieving a gradient structure in which the content of the low-melting-point alloy elements gradually decreases from the core to the outside of the disk body, while not flowing out too much to affect the structural strength of the disk body.
[0046] A hot pressing shaping method for a ceramic reinforced aluminum-based composite brake disc body according to one embodiment includes the following steps S110 to S130:
[0047] S110. Provide a ceramic-reinforced aluminum-based composite brake disc body to be hot-pressed and shaped.
[0048] In this embodiment, the ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped is prepared by the following method:
[0049] S1101. Provide ceramic reinforced aluminum matrix composite materials.
[0050] In this embodiment, the ceramic reinforced aluminum-based composite material is composed of 40% to 60% by mass of ceramic particles and the remainder of aluminum alloy.
[0051] The aluminum alloy is composed of 1% to 4% by mass of copper, 1% to 4% by mass of magnesium and the balance of aluminum, and is represented by Al-(1-4)Cu-(1~4)Mg.
[0052] It should be noted that since Cu and Mg are alloy elements that can form a low melting point eutectic component, the low melting point alloy elements in the present embodiment are Cu and Mg.
[0053] S1102, pressing the ceramic reinforced aluminum-based composite material into shape, and then sintering it.
[0054] In the present embodiment, the pressure of the press molding is 150 MPa to 300 MPa, and the holding time is 10 s to 30 s.
[0055] In this embodiment, the sintering temperature is 580° C. to 640° C., the sintering time is 1 to 1.5 hours, and the heating rate is 5° C. / min to 10° C. / min.
[0056] S120, provide Figure 1 and 2 The hot pressing shaping mold shown.
[0057] S130, placing the ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped in the third part 130 of the hot-pressing and shaped mold, and performing hot-pressing and shaped after closing the mold.
[0058] In the present embodiment, the temperature of the hot press forming is between the solidus and liquidus of the aluminum alloy.
[0059] Furthermore, the pressure of hot pressing shaping is 150MPa to 300MPa.
[0060] The above-mentioned hot pressing shaping method of the ceramic reinforced aluminum-based composite brake disc body is as follows: the ceramic reinforced aluminum-based composite brake disc body to be hot pressed is placed in the third part 130 of the hot pressing shaping mold, and hot pressing is performed after the mold is closed. The low-melting point alloy elements in the disc body form a liquid phase after reaching the eutectic point, and flow into the first annular area 112 through the second annular areas 122 on both sides. As the first annular area 112 is gradually filled, the speed and amount of the liquid phase outflow will gradually decrease, thereby achieving a gradient structure in which the content of the low-melting point alloy elements in the disc body decreases from the core to the outside, thereby ensuring both the temperature resistance of the disc surface and the structural strength of the disc body.
[0061] The following are specific embodiments.
[0062] Example 1
[0063] The method of steps S110 to S130 is used to hot press and shape a ceramic reinforced Al-(1-4)Cu-(1-4)Mg composite brake disc body with a ceramic particle mass content of 50%. The surface of the brake disc body after shaping has no plowing grooves when braked at 500°C, and the structural strength of the disc body is above 350MPa.
[0064] Comparative Example 1
[0065] Comparative Example 1 is substantially the same as Example 1, except that in Comparative Example 1, too many first annular areas 112 and second annular areas 122 are provided on each side.
[0066] The results showed that the structural strength of the disk was insufficient, which might be caused by excessive outflow of low-melting-point alloy elements.
[0067] Example 2
[0068] The method of steps S110 to S130 is used to hot press and shape a ceramic reinforced Al-(1-4)Cu-(1-4)Mg composite brake disc body with a ceramic particle mass content of 40%. The surface of the brake disc body after shaping has no plowing grooves when braked at 450°C, and the structural strength of the disc body is above 370MPa.
[0069] Example 3
[0070] The method of steps S110 to S130 is used to hot press and shape a ceramic reinforced Al-(1-4)Cu-(1-4)Mg composite brake disc body with a ceramic particle mass content of 60%. The surface of the brake disc body after shaping has no plowing grooves when braked at 550°C, and the structural strength of the disc body is above 340MPa.
[0071] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A hot pressing shaping method for a ceramic reinforced aluminum-based composite brake disc body, characterized in that: The following steps are involved: Providing a ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped; A hot pressing shaping mold is provided, the hot pressing shaping mold comprising an upper mold, a lower mold and a female mold, the upper mold and the lower mold are enclosed in the female mold to form a shaping cavity after the mold is closed, the shaping cavity comprises a first part, a second part and a third part, the shape of the third part corresponds to the ceramic reinforced aluminum-based composite brake disc body to be hot pressed and shaped, the second part comprises a plurality of second annular areas symmetrically arranged on the upper and lower sides of the third part and equidistantly spaced in the radial direction, the first part comprises a plurality of first annular areas symmetrically arranged on the opposite sides of the second part and equidistantly spaced in the radial direction, and the first annular areas on each side are respectively connected to the third part through the second annular areas on the respective sides; The ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped is placed in the third part of the hot-pressing and shaped mold, and hot-pressing and shaped are performed after the mold is closed.
2. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 1, characterized in that: The second annular zones on each side are equally spaced at a distance of 10 mm to 20 mm in the radial direction; the ring width of each second annular zone gradually decreases from the direction away from the third part to the direction close to the third part; the average ring width of each second annular zone is 5 μm to 10 μm; the axial height of each second annular zone is 3 mm to 5 mm.
3. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 1, characterized in that: The first annular zones on each side are equally spaced at a distance of 10 mm to 20 mm in the radial direction; the ring width of each first annular zone gradually decreases from the direction away from the third part to the direction close to the third part; the average ring width of each first annular zone is 3 mm to 5 mm; the axial height of each first annular zone is 3 mm to 5 mm.
4. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 1, characterized in that: There are 4 to 8 first annular areas on each side.
5. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to any one of claims 1 to 4, characterized in that: The ceramic reinforced aluminum-based composite brake disc body to be hot-pressed and shaped is prepared by the following method: Provide ceramic reinforced aluminum matrix composite materials; The ceramic reinforced aluminum-based composite material is pressed into shape and then sintered.
6. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 5, characterized in that: Calculated by mass percentage, the ceramic reinforced aluminum-based composite material consists of 40% to 60% of ceramic particles and the remainder of aluminum alloy.
7. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 6, characterized in that: Calculated by mass percentage, the aluminum alloy consists of 1% to 4% copper, 1% to 4% magnesium and the balance aluminum.
8. The hot pressing shaping method of a brake disc body according to claim 7, characterized in that: The temperature of the hot pressing shaping is between the solidus and liquidus of the aluminum alloy, and the pressure is 150MPa to 300MPa.
9. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 5, characterized in that: The pressing pressure is 150 MPa to 300 MPa, and the holding time is 10 s to 30 s.
10. The hot pressing shaping method of a ceramic reinforced aluminum-based composite brake disc body according to claim 5, characterized in that: The sintering temperature is 580° C. to 640° C., the sintering time is 1 to 1.5 hours, and the heating rate is 5° C. / min to 10° C. / min.