A method for recovering valuable metals from waste lithium iron phosphate positive electrode

Through the one-step carbothermal chlorination method and the two-stage quenching and condensation process, the problem of excessive use of acid and alkali liquids when recycling valuable metals in waste lithium-ion batteries is solved, achieving efficient and environmentally friendly metal recycling, and improving recycling efficiency and economic benefits.

CN117550628BActive Publication Date: 2024-10-29CHENZHOU HUINENG ENERGY STORAGE MATERIALS ENG RES CENT CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311510539.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-10-29
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

Existing technology requires the use of large amounts of acid and alkali liquids when recycling valuable metals in used lithium-ion batteries, resulting in environmental pollution and low metal recovery rates.

Method used

The one-step carbothermal chlorination method combined with the two-stage quenching and condensation process is used to recover lithium, iron and aluminum respectively through high-temperature roasting and quenching and condensation separation devices. This avoids the use of acid, alkali reagents or extraction solvents, shortens the process flow and increases the recovery rate.

Benefits of technology

It significantly improves the recovery rate of lithium and aluminum, reduces the equipment footprint and wastewater treatment burden, and has good environmental and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117550628B_ABST
    Figure CN117550628B_ABST
Patent Text Reader

Abstract

A method for recovering valuable metals from waste lithium iron phosphate positive electrodes, the method comprising discharging and disassembling waste lithium iron phosphate batteries, crushing and high-temperature treating the lithium iron phosphate positive electrode sheets obtained by disassembly, evenly mixing the high-temperature treated products with carbon materials and then subjecting them to roasting treatment in a high-purity Cl2 atmosphere, and then quenching and sublimating the roasting gas phase products in stages, respectively recovering ferric chloride and aluminum chloride, immersing the roasting solid phase products in water and filtering to obtain a lithium chloride aqueous solution, and then adding sodium carbonate to precipitate to obtain lithium carbonate. The present invention adopts a one-step carbon thermal chlorination method combined with a two-stage quenching and sublimation process, which can avoid the use of acid when recovering valuable metals from lithium iron phosphate positive electrodes, and does not need to use a large amount of alkali solution or extractant to separate and recover chlorides step by step. The present invention has a high metal recovery rate, low comprehensive cost, and good economic benefits and social and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of recycling waste lithium-ion batteries, and in particular relates to a method for recycling valuable metals in waste lithium iron phosphate positive electrodes. Background Art

[0002] With the rapid growth of electronic consumer products and electric vehicles, especially the widespread use of lithium iron phosphate batteries in new energy vehicles in recent years, the number of waste and retired lithium-ion batteries has also shown an explosive growth trend. Lithium-ion batteries contain valuable metals such as lithium, aluminum, and iron. How to reasonably recycle and reuse waste lithium-ion batteries is an urgent problem to be solved. At present, the methods for treating waste lithium-ion batteries mainly include wet processes and pyroprocesses, among which wet processes or pyroprocess-assisted wet processes are the main technical routes. However, the wet recovery process is to leaching and extracting the valuable metals in the positive electrode material, which requires the use of a large amount of acid and alkali solution. In addition, the process has many leaching steps, long leaching time, and low leaching rate. In addition, the large-scale use of acid and alkali also brings great pressure to environmental protection.

[0003] In order to avoid the large-scale use of acid and alkali in the metal leaching stage, the existing technologies CN115149134A, CN116759686 A, CN103060567A, CN112342394A, etc. use high-temperature chlorination roasting methods to chlorinate the metals in the positive electrode active material under high temperature and chlorine atmosphere, and then recover each metal step by step. However, the above methods need to be precipitated or solvent extracted to achieve the step-by-step recovery of metal chlorides, and there is still a large amount of consumption of alkaline reagents or extractants, as well as metal loss in the step-by-step recovery process, which reduces the recovery rate of valuable metals. Summary of the invention

[0004] In view of the above technical problems, the present invention adopts a one-step carbon thermal chlorination method combined with a two-stage quenching and sublimation process, which can avoid the use of acid, alkali reagents or extraction solvents when recovering valuable metals, and has good environmental benefits. In addition, the present invention has the advantages of short process flow, outstanding economic benefits, high recovery rate of valuable metals, low comprehensive recovery cost, etc.

[0005] To achieve the above object, the present invention provides a method for recovering valuable metals from waste lithium iron phosphate positive electrodes, which comprises the following steps in sequence:

[0006] (1) Discharging and disassembling waste lithium iron phosphate batteries to obtain lithium iron phosphate positive electrode sheets;

[0007] (2) crushing the lithium iron phosphate positive electrode sheet, and then treating it at high temperature in an air atmosphere;

[0008] (3) The product obtained by high temperature treatment is evenly mixed with the carbon material by ball milling, and then transferred to a sintering device, the sintering device is evacuated, high-purity Cl2 is introduced, and the temperature is increased and roasted in a Cl2 atmosphere;

[0009] (4) The gaseous product generated in the roasting process is sequentially passed through a quenching and de-sublimation separation device 1 and a quenching and de-sublimation separation device 2; the heat exchange tube of the quenching and de-sublimation separation device 1 contains SiCl4 preheated to 220° C.-240° C. and flowing in the countercurrent to the gaseous product, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 1; the heat exchange tube of the quenching and de-sublimation separation device 2 contains SiCl4 preheated to 100° C.-120° C. and flowing in the countercurrent to the gaseous product, and the condensed AlCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 2;

[0010] (5) The solid phase product obtained by roasting in step (3) is immersed in water, stirred and filtered to obtain a LiCl aqueous solution, and sodium carbonate is added to the LiCl aqueous solution to recover the precipitate to obtain Li2CO3.

[0011] Furthermore, in step (2), the average particle size of the lithium iron phosphate positive electrode sheet after crushing is less than or equal to 3 mm.

[0012] Furthermore, the heating rate of the high temperature treatment in step (2) is 5-10°C / min, the treatment temperature is 400-600°C, and the holding time is 3-6h;

[0013] Furthermore, the carbon material in step (3) is at least one of graphite, carbon black, carbon fiber, carbon nanotube and amorphous carbon.

[0014] Furthermore, the mass ratio of the product obtained by high temperature treatment in step (3) to the carbon material is 10:1-5:1.

[0015] Furthermore, the introduction rate of high-purity Cl2 in step (3) is 10-50 mL / min.

[0016] Furthermore, the calcination in step (3) is a two-stage calcination, the heating rate of the first stage is 3-5°C / min, the calcination temperature is 180-300°C, and the heat preservation is 1-3h, and the heating rate of the second stage is 5-10°C / min, the calcination temperature is 350-550°C, and the heat preservation is 3-6h.

[0017] Furthermore, in step (4), before SiCl4 is introduced into the heat exchange tube of the quenching and sublimation separation device (2), it is first preheated to 100°C-120°C, and the flow rate of SiCl4 in the heat exchange tube of the quenching and sublimation separation device (2) is 5-10mL / min. Furthermore, in step (4), before SiCl4 is introduced into the heat exchange tube of the quenching and sublimation separation device (1), it is first preheated to 220°C-240°C, and the flow rate of SiCl4 in the heat exchange tube of the quenching and sublimation separation device (1) is 5-10mL / min. Furthermore, in step (5), the water used for water immersion is deionized water; the time for water immersion stirring is 1-4h.

[0018] The beneficial effects of the present invention are as follows:

[0019] The present invention adopts a one-step carbon thermal chlorination method combined with a two-stage quenching and sublimation process to recover the lithium iron phosphate positive electrode, and utilizes the different boiling points of chlorides (LiCl, FeCl3 and AlCl3) generated by the carbon thermal chlorination reaction (see Table 1 below) to respectively recover lithium carbonate, ferric chloride and aluminum chloride, thereby avoiding the metal loss caused by the step-by-step recovery of the mixed chloride solid phase product, and significantly improving the recovery rate of lithium metal and aluminum metal; compared with the prior art, the present invention does not need to use a large amount of alkali solution or extractant to separate and recover chlorides step by step, thereby improving the metal recovery rate, shortening the process flow, saving equipment space, and reducing the burden of wastewater treatment, and has good economic benefits and social and environmental benefits.

[0020] Table 1

[0021] substance LiCl <![CDATA[FeCl3]]> <![CDATA[AlCl3]]> <![CDATA[SiCl4]]> Melting point(℃) 609 306 194 -70 Boiling point(℃) 1382 316 178 57.6 BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Flow chart of recycling valuable metals from waste lithium iron phosphate positive electrodes used in the embodiment of the present invention

[0023] Figure 2 Schematic diagram of recycling valuable metals from waste lithium iron phosphate positive electrodes used in an embodiment of the present invention

[0024] Figure 3 Schematic diagram of the quenching sublimation separation device of the present invention

[0025] Reference numerals:

[0026] 1, 2: Quenching and sublimation separation device;

[0027] 3, 4: Preheating device

[0028] 5: Calcination of solid phase products

[0029] 6: Quenching and sublimation separation device heat exchange tube

[0030] 7: Quenching and sublimation separation device deposition chamber DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to Examples and Comparative Examples.

[0032] Example 1

[0033] This embodiment includes the following steps:

[0034] Discharge and disassemble the waste lithium iron phosphate battery to obtain a lithium iron phosphate positive electrode sheet; directly crush the obtained lithium iron phosphate positive electrode sheet to particles with an average particle size of less than or equal to 3 mm, and then place the material in a muffle furnace, and treat it at a high temperature of 500°C for 3 hours at a heating rate of 5°C / min in an air atmosphere to remove the polymer binder and residual electrolyte lithium salt; ball-mill the product obtained by high-temperature treatment with graphite (the mass ratio of the two is 5:1) and mix them evenly, and then transfer the mixed material into a tubular furnace, evacuate the tubular furnace, and then introduce high-purity Cl2 at a flow rate of 30 mL / min, and heat and roast in a Cl2 atmosphere, and the roasting process is divided into two stages: the first stage is heated to 300°C at 5°C / min and kept warm for 1 hour, and the second stage is heated to 550°C at 5°C / min and kept warm for 3 hours;

[0035] The gaseous products generated during the roasting process are sequentially passed through a quenching and de-sublimation separation device 1 and a quenching and de-sublimation separation device 2; the heat exchange tube of the quenching and de-sublimation separation device 1 contains SiCl4 preheated to 220°C, with a flow rate of 5 mL / min and flowing in the reverse direction to the gaseous products, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 1; the heat exchange tube of the quenching and de-sublimation separation device 2 contains SiCl4 preheated to 120°C, with a flow rate of 5 mL / min and flowing in the reverse direction to the gaseous products, and the condensed AlCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 2;

[0036] The solid phase product obtained by roasting was immersed in deionized water and stirred for 1 hour, and the LiCl aqueous solution was obtained by suction filtration. Sodium carbonate was then added to the LiCl aqueous solution to recover the precipitate to obtain Li2CO3.

[0037] Example 2

[0038] This embodiment includes the following steps:

[0039] Discharge and disassemble the waste lithium iron phosphate battery to obtain a lithium iron phosphate positive electrode sheet; directly crush the obtained lithium iron phosphate positive electrode sheet to particles with an average particle size of less than or equal to 3 mm, and then place the material in a muffle furnace, and treat it at a high temperature of 400°C for 6 hours at a heating rate of 10°C / min in an air atmosphere to remove the polymer binder and residual electrolyte lithium salt; ball-mill the product obtained by high temperature treatment with carbon black (the mass ratio of the two is 10:1) and mix them evenly, and then transfer the mixed material into a tubular furnace, evacuate the tubular furnace, and then introduce high-purity Cl2 at a flow rate of 10mL / min, and heat and roast in a Cl2 atmosphere, and the roasting process is divided into two stages: the first stage is heated to 180°C at 3°C / min and kept warm for 3 hours, and the second stage is heated to 450°C at 5°C / min and kept warm for 3 hours;

[0040] The gaseous products generated during the roasting process are sequentially passed through a quenching and de-sublimation separation device 1 and a quenching and de-sublimation separation device 2; the heat exchange tube of the quenching and de-sublimation separation device 1 contains SiCl4 preheated to 240°C, with a flow rate of 10 mL / min and in a countercurrent flow to the gaseous products, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 1; the heat exchange tube of the quenching and de-sublimation separation device 2 contains SiCl4 preheated to 100°C, with a flow rate of 10 mL / min and in a countercurrent flow to the gaseous products, and the condensed AlCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 2;

[0041] The solid phase product obtained by roasting was immersed in deionized water and stirred for 4 hours, and the LiCl aqueous solution was obtained by suction filtration. Sodium carbonate was then added to the LiCl aqueous solution to recover the precipitate to obtain Li2CO3.

[0042] Example 3

[0043] This embodiment includes the following steps:

[0044] Discharge and disassemble the waste lithium iron phosphate battery to obtain a lithium iron phosphate positive electrode sheet; directly crush the obtained lithium iron phosphate positive electrode sheet to particles with an average particle size of less than or equal to 3 mm, and then place the material in a muffle furnace, and treat it at a high temperature of 600°C for 3 hours at a heating rate of 10°C / min in an air atmosphere to remove the polymer binder and residual electrolyte lithium salt; ball-mill the product obtained by high temperature treatment with carbon fiber (the mass ratio of the two is 10:1) and mix them evenly, and then transfer the mixed material into a tubular furnace, evacuate the tubular furnace, and then pass high-purity Cl2 at a flow rate of 50mL / min, and heat and roast in a Cl2 atmosphere. The roasting process is divided into two stages: the first stage is heated to 250°C at 5°C / min and kept warm for 2 hours, and the second stage is heated to 350°C at 10°C / min and kept warm for 6 hours;

[0045] The gaseous products generated during the roasting process are sequentially passed through a quenching and de-sublimation separation device 1 and a quenching and de-sublimation separation device 2; the heat exchange tube of the quenching and de-sublimation separation device 1 contains SiCl4 preheated to 230°C, with a flow rate of 10 mL / min and flowing in the reverse direction to the gaseous products, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 1; the heat exchange tube of the quenching and de-sublimation separation device 2 contains SiCl4 preheated to 110°C, with a flow rate of 10 mL / min and flowing in the reverse direction to the gaseous products, and the condensed AlCl3 is recovered in the deposition chamber of the quenching and de-sublimation separation device 2;

[0046] The solid phase product obtained by roasting was immersed in deionized water and stirred for 3 hours, and the LiCl aqueous solution was obtained by suction filtration. Sodium carbonate was then added to the LiCl aqueous solution to recover the precipitate to obtain Li2CO3.

[0047] Comparative Example

[0048] Discharge and disassemble the waste lithium iron phosphate battery to obtain a lithium iron phosphate positive electrode sheet; directly crush the obtained lithium iron phosphate positive electrode sheet to particles with an average particle size of less than or equal to 3 mm, and then place the material in a muffle furnace, and treat it at a high temperature of 500°C for 3 hours at a heating rate of 5°C / min in an air atmosphere to remove the polymer binder and residual electrolyte lithium salt; ball-mill the product obtained by high-temperature treatment with graphite (the mass ratio of the two is 5:1) and mix them evenly, and then place the mixed material in a tubular furnace, evacuate the tubular furnace, and then pass high-purity Cl2 at a flow rate of 30 mL / min, and heat and roast in a Cl2 atmosphere, and the roasting process is to heat to 300°C at a rate of 5°C / min and keep warm for 4 hours;

[0049] Passing the gas phase product generated during the roasting process through a condensation device, and recovering AlCl3 in the condensation device;

[0050] The solid phase product obtained by roasting was immersed in deionized water and stirred for 1 hour, and a mixed chloride metal salt aqueous solution containing LiCl and FeCl3 was obtained by suction filtration, and ammonia water was added to the mixed chloride metal salt aqueous solution to adjust the pH of the solution to 3.5, and iron hydroxide precipitate and filtrate were obtained by suction filtration;

[0051] Then, sodium carbonate is added to the filtrate to recover the precipitate to obtain Li2CO3.

[0052] Recovery test:

[0053] The recovery rate is calculated by the formula: Recovery rate = actual product mass / theoretical product mass × 100%, wherein the theoretical product mass is obtained by determining the content of each element in the crushed product of the lithium iron phosphate positive electrode sheet by the ICP method, and calculating the theoretical mass value of the complete conversion into the product.

[0054] The test results of the recovery rates of each element in Examples 1-3 and Comparative Examples are shown in Table 2 below:

[0055] Table 2

[0056] Li(%) Fe(%) Al(%) Example 1 99.3 97.2 95.6 Example 2 98.6 97.8 94.3 Example 3 98.8 96.9 96.2 Comparative Example 71.6 82.6 94.5

[0057] As can be seen from Table 2, compared with the comparative example, Examples 1-3 can significantly improve the recovery rate of Li because there is no need to recover the mixed chloride salt of Li and Fe step by step. In addition, the recovery rates of Fe and Al metals in Examples 1-3 are relatively high, reflecting that the recovery purity of lithium carbonate in Examples 1-3 is also better than that in the comparative example.

Claims

1. A method for recovering valuable metals from waste lithium iron phosphate positive electrodes, characterized in that: The following steps are included in sequence: (1) Discharging and disassembling waste lithium iron phosphate batteries to obtain lithium iron phosphate positive electrode sheets; (2) crushing the lithium iron phosphate positive electrode sheet, and then treating it at high temperature in an air atmosphere; (3) The product obtained by high temperature treatment is ball-milled and mixed with the carbon material, and then transferred to a sintering device, the sintering device is evacuated, high-purity Cl2 is introduced, and the temperature is increased and roasted in a Cl2 atmosphere; the introduction rate of the high-purity Cl2 is 10-50mL / min; the roasting is a two-stage roasting, the heating rate of the first stage roasting is 3-5°C / min, the roasting temperature is 180-300°C, and the heat preservation is 1-3h, and the heating rate of the second stage roasting is 5-10°C / min, the roasting temperature is 350-550°C, and the heat preservation is 3-6h; (4) the gaseous product generated in the roasting process is sequentially passed through a quenching and de-escalating device (1) and a quenching and de-escalating device (2); the heat exchange tube of the quenching and de-escalating device (1) contains SiCl4 preheated to 220°C-240°C and flowing in the countercurrent to the gaseous product, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-escalating device (1); the heat exchange tube of the quenching and de-escalating device (2) contains SiCl4 preheated to 100°C-120°C and flowing in the countercurrent to the gaseous product, and the condensed FeCl3 is recovered in the deposition chamber of the quenching and de-escalating device (2). The condensed AlCl3 is recovered in the deposition chamber; before SiCl4 is introduced into the heat exchange tube of the quenching and decondensing separation device (1), it is first preheated to 220°C-240°C, and the flow rate of SiCl4 in the heat exchange tube of the quenching and decondensing separation device (1) is 5-10mL / min; before SiCl4 is introduced into the heat exchange tube of the quenching and decondensing separation device (2), it is first preheated to 100°C-120°C, and the flow rate of SiCl4 in the heat exchange tube of the quenching and decondensing separation device (2) is 5-10mL / min; (5) The solid phase product obtained by roasting in step (3) is immersed in water, stirred and filtered to obtain a LiCl aqueous solution, and sodium carbonate is added to the LiCl aqueous solution to recover the precipitate to obtain Li2CO3.

2. The method according to claim 1, characterized in that The average particle size of the lithium iron phosphate positive electrode sheet after crushing in step (2) is less than or equal to 3 mm.

3. The method according to claim 1, characterized in that The heating rate of the high temperature treatment in step (2) is 5-10°C / min, the treatment temperature is 400-600°C, and the insulation time is 3-6h.

4. The method according to claim 1, characterized in that The carbon material in step (3) is at least one of graphite, carbon black, carbon fiber, carbon nanotube and amorphous carbon.

5. The method according to claim 1, characterized in that The mass ratio of the product obtained by high temperature treatment in step (3) to the carbon material is 10:1-5:

1.

6. The method according to claim 1, characterized in that The water used for immersion in step (5) is deionized water; and the stirring time for immersion is 1-4 hours.

Citation Information

Patent Citations

  • Method for processing waste lithium ion battery positive plate to extract valuable metal

    CN103060567A

  • Incomplete extraction battery recovery method

    CN112342394A

  • Method and equipment for high-temperature chloridizing roasting of waste lithium battery and application

    CN115149134A

  • Method for recovering valuable metal from lithium iron phosphate battery positive electrode material

    CN116759686A

  • Method for treating precious metal iron trapped material

    CN113278803A