A method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization and its application

Through thermal degradation and free radical polymerization technology, a polyolefin microsphere emulsion with high grafting rate and low dispersant content is prepared, which solves the problems of air permeability and internal resistance of lithium battery separators caused by high dispersant content in the existing technology, and significantly Improved the stability and life of lithium batteries.

CN117586529BActive Publication Date: 2024-10-01GUANGDONG CARBON LANGUAGE NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311554009.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-21
Publication Date
2024-10-01
Estimated Expiration
2043-11-21

AI Technical Summary

Technical Problem

The existing technology requires a high content of dispersant when preparing polyolefin microsphere emulsion, which results in increased air permeability, increased internal resistance and affected stability of the lithium battery separator. It is difficult to effectively reduce the dispersant content to improve the stability and life of the lithium battery.

Method used

Using a method based on thermal degradation and free radical polymerization, the polyolefin is thermally degraded by raising the temperature under nitrogen protection, and free radical polymerization is performed with acrylate monomers in the molten state, and then a very small amount of dispersant is added to form a stable Narrow size distribution polyolefin microsphere emulsion.

Benefits of technology

A polyolefin microsphere emulsion with high grafting rate (more than 98%) and low dispersant content (0.1%-0.2%) is achieved, which significantly improves the uniformity of microsphere particle size and bonding strength and avoids clogging and battery The problem of increased internal resistance extends the cycle life of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117586529B_ABST
    Figure CN117586529B_ABST
Patent Text Reader

Abstract

The present invention provides a method and application for preparing polyolefin microspheres based on thermal degradation and free radical polymerization, and belongs to the technical field of preparing polyolefin microspheres. The method adds waste polyolefin to a stirred reactor, heats up, and drips acrylate monomers into the reaction system to perform free radical polymerization. After the dripping is completed, the monomers are polymerized for a certain period of time, and the polyolefin material modified by acrylate polymers is obtained by precipitation. Then, the above-mentioned materials are pulverized to obtain polyolefin powder. The polyolefin powder is added to a pressure reactor, heated and melted, and then a dispersant and water are added under stirring, and stirred for a certain period of time to obtain a polyolefin microsphere emulsion. The surface of the polymer microsphere has an acrylate polymer itself with a certain dispersion and bonding ability, which can greatly reduce the amount of dispersant (0.1%-0.2%) on the one hand, and on the other hand, the problem of pore blocking and increased internal resistance of the battery caused by the emulsifier is avoided to a great extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste polymer upgrading and recycling and polyolefin microsphere emulsion preparation, and specifically relates to a method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization and application thereof. Background Art

[0002] At present, with the widespread use of synthetic polymers in various fields, while bringing us convenience, the accumulation of a large amount of waste plastics in the natural environment has caused serious white pollution problems. How to solve the growing problem of waste plastic pollution to the environment and realize the recycling and reuse of waste plastics is a major scientific and technological problem facing today's society and a challenge for my country to achieve sustainable development. At present, polyolefin polymer materials are the most widely used type of polymer materials in the world, such as polyethylene, and the world production capacity is expected to reach 125 million tons by 2025. Polyolefin materials generally include polyethylene, poly-1-butene, polypropylene, and their copolymers. How to efficiently recycle waste polyolefins and make high-value use of them has always been a research hotspot.

[0003] Polyolefin microspheres, as coating materials for diaphragms, can play an adhesive role in the field of lithium battery diaphragm coating. Since the polyolefin molecular chain has very weak polarity and extremely strong hydrophobicity, it is necessary to add more than 10wt% of dispersant or emulsifier to stabilize the polyolefin microsphere emulsion when preparing the polyolefin microsphere emulsion. Unfortunately, the addition of a large amount of dispersant can easily cause diaphragm pore blockage during the coating process, causing the diaphragm permeability to increase, which in turn leads to an increase in the internal resistance of the battery and affects the stability of the lithium battery. In order to solve the impact of dispersants on the stability and life of lithium batteries, it is urgent to find a simple and effective method for preparing polyolefin microspheres with a reduced dispersant content.

[0004] At present, there are reports on the preparation method of polyolefin microsphere emulsion with low dispersant content. The patent with publication number CN115926195B provides a preparation method and application of polyolefin microsphere emulsion with dispersant content less than 0.5%. This method performs surface oxidation treatment on polyolefin, and then prepares polyolefin microsphere emulsion by emulsion polymerization. The polyolefin microsphere emulsion is spray-dried to obtain polyolefin microsphere powder, and then the polyolefin microsphere powder is added with a dispersant to obtain polyolefin microsphere emulsion. This method prepares acrylate-modified polyolefin powder only by polymerization reaction on the surface of the original powder, and the morphology of the microsphere can only be controlled by the morphology of the original powder. In addition, the grafting rate of the polyolefin surface oxidation-emulsion polymerization method is low and the monomer conversion rate is low. It is necessary to explore a more accurate method to prepare acrylate-modified polyolefin powder, control the size of polymer spheres, and further prepare polyolefin microspheres with low dispersant content. Summary of the invention

[0005] The present invention discloses a method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization and its application. In the process of preparing polyolefin microspheres, only a very small amount of dispersant needs to be added to form a stably dispersed polyolefin microsphere emulsion with a narrow size distribution, and the grafting rate is as high as more than 98%. The microsphere emulsion can be used to prepare lithium battery separator coating materials.

[0006] The present invention first provides a method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization, comprising:

[0007] Add waste polyolefin into a stirred reactor, heat it to 250-370°C under nitrogen protection and react for 4-8 hours; then, drop acrylate monomer into the reaction system to carry out free radical polymerization, and after the drop addition, react for 2-6 hours to obtain acrylate polymer modified polyolefin material through precipitation; then, pulverize the above acrylate polymer modified polyolefin material to obtain polyolefin powder; add the polyolefin powder into a pressure reactor, heat it to melt, add dispersant and water under stirring, and stir for a certain time to obtain polyolefin microsphere emulsion.

[0008] Preferably, the polyolefin comprises a homopolymer or copolymer of waste polyethylene, poly-1-butene, or polypropylene.

[0009] Preferably, the acrylic esters include one or more of acrylate, methyl methacrylate, ethyl acrylate, acrylic acid or methacrylic acid.

[0010] Preferably, the amount of the dispersant is 0.1%-0.2%.

[0011] Preferably, the dispersant is one or both of anionic dispersants and nonionic dispersants.

[0012] Preferably, the anionic dispersant is an alkyl sulfonate, an alkyl sulfate or a phosphate; and the nonionic dispersant is polyvinyl alcohol, polyoxypropylene ether or polyol fatty acid ester.

[0013] Preferably, the mass ratio of the polyolefin powder to the acrylic monomer is 1:(0.01-0.05).

[0014] Preferably, the polyolefin powder is added into a pressure reactor, the temperature in the reactor is 130-150° C., the stirring speed is 1000-1500 r / min, and the stirring time is 2-3 h.

[0015] The present invention also provides the micro-nano polyolefin microsphere emulsion obtained by the above preparation method.

[0016] The present invention also provides application of the polyolefin microsphere emulsion in preparing a lithium battery coating diaphragm.

[0017] Beneficial Effects of the Invention

[0018] The present invention discloses a method and application of preparing polyolefin microspheres based on thermal degradation and free radical polymerization, wherein the polyolefin microspheres are derived from the thermal degradation and free radical polymerization of waste polyolefins. Since the polyolefin is in a molten state during the grafting process of acrylate, its free radical polymerization is carried out at the molecular level, the grafting rate is as high as 98% or more, and its acrylate is more evenly dispersed in the polyolefin system. Due to the uniformity of dispersion and high grafting rate of acrylate polymers, and the use of high-temperature melt dispersion emulsification in the preparation of polyolefin microsphere emulsions, the particle size of the polyolefin microspheres is more uniform, and the median particle size is controlled between 1.0um-4.0um; at the same time, the amount of dispersant used when the emulsion is stable is further reduced to as low as 0.1%-0.2%. The coated diaphragm formed by coating the microsphere emulsion prepared by this method has good bonding strength with the positive and negative electrode sheets, while avoiding the problems of pore blocking, black spot lithium precipitation, increased battery internal resistance, and insufficient cycle life caused by a large amount of dispersants.

[0019] Compared with the prior art, the present invention realizes the high-value utilization of waste polymers. Secondly, only 0.1-0.2% of dispersant is used in the preparation process, which is 1% of the polyolefin microsphere emulsion dispersant currently used in the market. At the same time, the surface of the microspheres is covered with acrylic polymers or oligomers, which have a certain bonding ability, greatly reducing the amount of adhesives, dispersants, and wetting agents used during coating, which not only saves material costs, but also avoids the problems of pore blockage and increased internal resistance of the battery caused by adhesives and dispersants. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The particle size and particle size distribution diagram of the polyolefin microemulsion prepared in Examples 1-4 of the present invention;

[0021] Figure 2 The particle size and particle size distribution diagram of the polyolefin microemulsion prepared in Comparative Examples 1-4. DETAILED DESCRIPTION

[0022] The present invention first provides a method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization, comprising:

[0023] Add the waste polyolefin into a stirred reactor, and heat it to 250-370°C under nitrogen protection to react for 4-8 hours; then, drop the acrylate monomer into the reaction system to perform free radical polymerization. After the dropwise addition is completed, react for another 2-6 hours, pour the reaction solution into ethanol while hot to precipitate, and obtain a polyolefin material modified by an acrylate polymer; then, subject the polyolefin material modified by the acrylate polymer to a pulverization treatment, wherein the pulverization treatment is preferably to grind the polyolefin material by liquid nitrogen freezing, sieve, and pulverize the polyolefin material to obtain a polyolefin powder, and add the polyolefin powder into a pressure reactor, and control the temperature in the reactor to preferably 120-200°C, more preferably 130-150°C, and the stirring speed is preferably 300-1500r / min, more preferably 1000-1500r / min, and the stirring time is preferably 1-4h, more preferably 2-3h.

[0024] The polyolefin microsphere emulsion can be obtained.

[0025] According to the present invention, the waste polyolefin raw material is first added to a stirred reactor, and the temperature is raised to 250-370°C for reaction for 4-8 hours under nitrogen protection, and the polyolefin material with different acrylic monomers and modified content is prepared by adjusting the reaction temperature and adding the content of acrylic ester monomers. The source of the waste polyolefin raw material is commercially available, and preferably includes homopolymers or copolymers of waste polyethylene, waste poly-1-butene, and waste polypropylene. The specific method is preferably: for waste polyethylene or poly-1-butene, the reaction temperature is 250°C-300°C; for polypropylene, the reaction temperature is 320-370°C; in the process of melt thermal degradation, a free radical graft polymerization reaction of acrylic ester monomers is carried out on the side chain or end of the polyolefin, so that the surface hydrophilicity is greatly increased, and the amount of dispersant used when the polymer microspheres are stable in the emulsion is greatly reduced.

[0026] According to the present invention, the content of the dispersant is 0.1%-0.2%. The dispersant is preferably one or both of anionic emulsifiers or nonionic emulsifiers. Among them, the anionic dispersant is alkyl sulfonate, alkyl sulfate, phosphate; the nonionic dispersant is polyvinyl alcohol, polyoxypropylene ether, polyol fatty acid ester. More preferably, it is a combination of sodium dodecylbenzene sulfonate and polyethylene oxide, and the mass ratio is preferably 1:1.

[0027] According to the present invention, the acrylic acid ester monomer preferably includes one or more of acrylic acid ester, methyl methacrylate, ethyl acrylate, acrylic acid or methacrylic acid. The present invention generates active free radicals by melt thermal degradation, and grafts a layer of polyacrylate polymer on the side chain or end of polyolefin to form polyolefin microspheres with core-shell structure. At the same time, the acrylic acid ester polymer itself has a certain bonding ability. The polyolefin microsphere separator prepared by this method has good bonding strength with the positive and negative electrodes, and avoids the use of a large amount of emulsifiers, adhesives, dispersants, wetting agents, etc., and avoids the problems of short battery life caused by pore blockage and increased battery internal resistance.

[0028] According to the present invention, the mass ratio of the polyolefin to the acrylic monomer is preferably 1:

[0029] (0.003-0.02), more preferably 1:(0.01-0.02).

[0030] According to the present invention, the solid content of the polyolefin microsphere emulsion is 10%-40%.

[0031] The present invention also provides a micro-nano polyolefin microsphere emulsion obtained by the above preparation method. In the polyolefin microsphere emulsion, the particle size of the microsphere is 1um-2um.

[0032] The present invention also provides the use of the polyolefin microsphere emulsion in preparing a lithium battery coating diaphragm.

[0033] The preparation method of the polyolefin microsphere emulsion coated diaphragm of the present invention is as follows:

[0034] Step 1, preparing slurry: adding polyolefin microsphere emulsion into water, and adding adhesive, wetting agent and other additives in sequence, stirring to form a uniform coating liquid;

[0035] Step 2, coating experiment: coating the prepared coating solution on one or two surfaces of the lithium battery / sodium battery / supercapacitor separator;

[0036] Step three, drying treatment: drying the coated diaphragm to obtain the polyolefin microsphere coated diaphragm.

[0037] According to the present invention, there is no special restriction on the auxiliary agents such as the adhesive and the wetting agent, and they are selected according to the conventional types in the art. The adhesive is preferably one or more of polyacrylic acid, polyacrylate, polyacrylonitrile and its modified copolymer, polypropylene and its modified copolymer, and polyurethane; the wetting agent is preferably one or more of polyether, polyethylene oxide and its modified copolymer, and fluorine-containing polymer. The mass ratio of the polyolefin microsphere emulsion, the adhesive, and the wetting agent is preferably (65-95): (0.1-20): (1-5).

[0038] The present invention is further described in detail below with reference to specific examples. The raw materials involved in the examples are all commercially available without special requirements.

[0039] Example 1

[0040] 500g of waste polyethylene raw material was added to a stirred reactor. Under nitrogen protection, the temperature was raised to 270℃ for reaction for 4 hours. Then 7.5g of methyl methacrylate was slowly added through the feed port to ensure that the dropping time was 1h. After the dropping was completed, the reaction was continued for 2h. While hot, the reaction solution was poured into ethanol for precipitation, filtered, and dried to obtain a polyolefin material modified with an acrylic ester polymer. The monomer conversion results are shown in Table 1. The above polyolefin material was placed in a liquid nitrogen environment for grinding, dispersion, and sieving to obtain a polyethylene powder modified with polymethyl methacrylate. The polyolefin powder was added to a high-temperature and high-pressure reactor. After heating and melting, the temperature was controlled at 140℃, the stirring speed was 1200r / min, 0.35g of polyethylene oxide and 0.35g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water were added. After stirring for 2 hours, a polyethylene microsphere emulsion was formed. The particle size and particle size distribution of the polyethylene microsphere emulsion were tested by a particle size analyzer. Figure 1 a and Table 2.

[0041] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0042] Example 2

[0043] 500g of waste polyethylene raw material was added to a stirred reactor. Under nitrogen protection, the temperature was raised to 270℃ for reaction for 4 hours. Then 7.5g of methacrylic acid was slowly added through the feed port to ensure that the dropping time was 1h. After the dropping was completed, the reaction was continued for 2h. While hot, the reaction solution was poured into ethanol for precipitation, filtered, and dried to obtain a polyolefin material modified by an acrylic polymer. The above polyolefin material was placed in a liquid nitrogen environment for grinding, dispersion, and sieving to obtain a polyethylene powder modified with polymethacrylic acid. The monomer conversion results are shown in Table 1. The polyolefin powder was added to a high-temperature and high-pressure reactor. After heating and melting, the temperature was controlled at 140℃, the stirring speed was 1200r / min, 0.35g of polyethylene oxide and 0.35g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water were added. After stirring for 2 hours, a polyethylene microsphere emulsion was formed. The particle size and particle size distribution of the polyethylene microsphere emulsion were tested by a particle size analyzer. Figure 1 b and Table 2.

[0044] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0045] Example 3

[0046] 500g of waste polypropylene raw material was added to a stirred reactor. Under nitrogen protection, the temperature was raised to 350℃ for reaction for 4 hours. Then 7.5g of methyl methacrylate was slowly added through the feed port to ensure that the dropping time was 1h. After the dropping was completed, the reaction was continued for 2h. While hot, the reaction solution was poured into ethanol for precipitation, filtered, and dried to obtain a polyolefin material modified with an acrylic ester polymer. The above polyolefin material was placed in a liquid nitrogen environment for grinding, dispersion, and sieving to obtain polymethyl methacrylate-modified polypropylene powder. The monomer conversion results are shown in Table 1. The polyolefin powder was added to a high-temperature and high-pressure reactor. After heating and melting, the temperature was controlled at 140℃, the stirring speed was 1200r / min, 0.35g of polyethylene oxide and 0.35g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water were added. After stirring for 2 hours, a polyethylene microsphere emulsion was formed. The particle size and particle size distribution of the polypropylene microsphere emulsion were tested by a particle size analyzer. Figure 1 c and Table 2.

[0047] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0048] Example 4

[0049] 500g of waste polypropylene raw material was added to a stirred reactor. Under nitrogen protection, the temperature was raised to 350℃ for reaction for 4 hours. Then 7.5g of methacrylic acid was slowly added through the feed port to ensure that the dropping time was 1h. After the dropping was completed, the reaction was continued for 2h. While hot, the reaction solution was poured into ethanol for precipitation, filtered, and dried to obtain a polyolefin material modified by an acrylic polymer. The above polyolefin material was placed in a liquid nitrogen environment for grinding, dispersion, and sieving to obtain polymethacrylic acid-modified polypropylene powder. The monomer conversion results are shown in Table 1. The polyolefin powder was added to a high-temperature and high-pressure reactor. After heating and melting, the temperature was controlled at 140℃, the stirring speed was 1200r / min, 0.35g of polyethylene oxide and 0.35g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water were added. After stirring for 2 hours, a polyethylene microsphere emulsion was formed. The particle size and particle size distribution of the polypropylene microsphere emulsion were tested by a particle size analyzer. Figure 1 d and Table 2.

[0050] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0051] Comparative Example 1

[0052] Add 500g of waste polyethylene raw material into a stirred reactor, and under nitrogen protection, heat it to 270℃ and react for 7 hours. Pour the reaction solution into ethanol while hot for precipitation, filter and dry to obtain a polyolefin material. Put the above polyolefin material into a liquid nitrogen environment for grinding, dispersion and sieving to obtain polyethylene powder. Add the polyolefin powder into a high-temperature and high-pressure reactor, heat it to melt, control the temperature at 140℃, stir at 1200r / min, add 25g of polyethylene oxide and 25g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water, stir for 2 hours to form a polyethylene microsphere emulsion. The particle size and particle size distribution of the polyethylene microsphere emulsion are tested by a particle size analyzer. Figure 2 a and Table 2.

[0053] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0054] Comparative Example 2

[0055] Add 500g of waste polypropylene raw material to a stirred reactor, and under nitrogen protection, heat it to 350℃ and react for 7 hours. Pour the reaction solution into ethanol while hot for precipitation, filter and dry to obtain a polyolefin material. Put the above polyolefin material into a liquid nitrogen environment for grinding, dispersion and sieving to obtain polypropylene powder. Add the polyolefin powder to a high-temperature and high-pressure reactor, heat it to melt, control the temperature at 140℃, stir at 1200r / min, add 25g of polyethylene oxide and 25g of sodium dodecylbenzene sulfonate dispersant, and 1250g of water, stir for 2 hours to form a polyethylene microsphere emulsion. The particle size and particle size distribution of the polypropylene microsphere emulsion are tested by a particle size analyzer. Figure 2 b and Table 2.

[0056] 100 g of the above-mentioned emulsion, 160 g of deionized water, 6 g of polyacrylic acid and 8 g of a polyether wetting agent were prepared together into a uniform coating liquid, which was coated on one surface of a 16 um lithium battery separator. After drying, a polyolefin microsphere-coated separator material was obtained. The test performance is shown in Table 3.

[0057] Comparative Example 3

[0058] The polyolefin microemulsion was prepared by referring to the preparation method of the patent publication number CN115926195B. The type and amount of the dispersant were 0.5% as reported in the patent, as follows: 500g of polyethylene powder was heated at 8000V / m 2 After surface oxidation treatment under the action of high-frequency high-voltage electricity, it was added to 2000g of water, and 1.25g of emulsifier polyoxyethylene ether was added. Under the protection of nitrogen, 7.5g of methyl methacrylate monomer was added dropwise, and the mixture was stirred at 82°C for 20min to carry out emulsion polymerization to obtain a polyolefin microsphere emulsion with a core-shell structure. The emulsion was atomized into small droplets in the air and contacted with 150°C hot air in a drying chamber for 2s. The high temperature instantly evaporated the water, and the droplets were dried into fine powder and fell to the bottom of the drying chamber to obtain polyolefin microsphere powder. The monomer conversion results are shown in Table 1. 2.5g of polyoxyethylene ether and 1250g of water were added to the polyolefin microsphere powder and stirred at 25°C for 30min to form an emulsion. The particle size and particle size distribution of this microsphere emulsion were tested by a particle size analyzer. Figure 2 c and Table 2.

[0059] 100 g of the above emulsion, 160 g of deionized water, 6 g of polyacrylic acid, and 8 g of a polyether wetting agent were prepared into a uniform coating solution, which was coated on one surface of a 16 um lithium battery separator, and dried to obtain a polyolefin microsphere coated separator. The test performance is shown in Table 3.

[0060] Comparative Example 4

[0061] Reference is made to the preparation method of the patent publication number CN115926195B, in which the type and amount of dispersant are consistent with those of this patent, as follows: 500g of polyethylene powder is heated at 8000V / m 2 After surface oxidation treatment under the action of high-frequency high-voltage electricity, it was added to 2000g of water, 1.25g of emulsifier polyoxyethylene ether was added, and 7.5g of methyl methacrylate monomer was added dropwise under the protection of nitrogen. The mixture was stirred at 82°C for 20min to carry out emulsion polymerization to obtain a polyolefin microsphere emulsion with a core-shell structure. The emulsion was atomized into small droplets in the air and contacted with 150°C hot air in a drying chamber for 2s. The high temperature instantly evaporated the water, and the droplets were dried into fine powder and fell to the bottom of the drying chamber to obtain polyolefin microsphere powder. The monomer conversion results are shown in Table 1. 0.35g of polyethylene oxide, 0.35g of sodium dodecylbenzene sulfonate dispersant and 1250g of water were added to the polyolefin microsphere powder and stirred at 25°C for 30min to form an emulsion. The particle size and particle size distribution of this microsphere emulsion were tested by a particle size analyzer. Figure 2 d and Table 2.

[0062] 100 g of the above emulsion, 160 g of deionized water, 6 g of polyacrylic acid, and 8 g of a polyether wetting agent were prepared into a uniform coating solution, which was coated on one surface of a 16 um lithium battery separator, and dried to obtain a polyolefin microsphere coated separator. The test performance is shown in Table 3.

[0063] Table 1 Results of monomer conversion of acrylate modified polyolefin powder

[0064] (The mass percentage of the grafted monomer amount of polyolefin to the theoretical grafted monomer amount, %)

[0065]

[0066] Table 2 Polyolefin microemulsion particle size and particle size distribution results

[0067] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Particle size D50(um) 1.04 1.01 1.04 1.01 3.45 1.96 1.72 1.14 Particle size D90(um) 1.60 1.56 1.65 1.56 10.72 11.25 3.84 5.28

[0068] Table 3 Test results of polyolefin microsphere coated diaphragm materials

[0069]

[0070]

[0071] In addition, 15 of the 100 batteries made in comparative example 1 had a capacity drop of 400 to 700 weeks, and 7 had a capacity of less than 70% after 1500 cycles; 8 soft-pack batteries were bulged, and 7 had black spots after disassembly; 18 of the 100 batteries made in comparative example 2 had a capacity drop of 400 to 700 weeks, and 10 had a capacity of less than 70% after 1500 cycles; 12 soft-pack batteries were bulged, and 10 had black spots after disassembly; 100 batteries made in comparative example 3 did not have a capacity drop, and the capacity was 81.8% after 1500 cycles; 10 of the 100 batteries made in comparative example 4 had a capacity drop of 400 to 700 weeks, and 85 had a capacity of 75.8% after 1500 cycles; 5 soft-pack batteries were bulged, and 2 had black spots after disassembly. In the same way, 100 batteries were made in Examples 1-4 of the present invention, and no water drop occurred. After 1500 cycles, the capacity did not drop below 85%, and no black spots or other defects were found after the batteries were disassembled. The preparation methods of Comparative Examples 3 and 4 are derived from the patent publication number CN115926195B, wherein the type and amount of dispersant in Comparative Example 3 are based on the original patent, and the type and amount of dispersant in Comparative Example 4 are based on the amount used in this patent. The performance of the two comparative examples is weaker than that of Examples 1-4 in all aspects.

[0072] The above results show that the separators of Examples 1-4 have lower air permeability and lower battery internal resistance, higher dry and wet adhesion strength with the pole pieces, and the battery still has a capacity retention rate of more than 85% after 1500 cycles.

[0073] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization, characterized in that: include: Add the waste polyolefin into a stirred reactor, heat to 250-370°C and react for 4-8 hours under nitrogen protection; Then, acrylic acid, methacrylic acid or methyl methacrylate is added dropwise to the reaction system to perform free radical polymerization. After the addition is completed, the reaction is continued for 2-6 hours, and a modified polyolefin material is obtained through precipitation. Then, the modified polyolefin material is subjected to a pulverization treatment to obtain a polyolefin powder. The polyolefin powder is added into a pressure reactor, heated and melted, and a dispersant and water are added under stirring, and stirred for a certain period of time to obtain a polyolefin microsphere emulsion. The waste polyolefins include homopolymers or copolymers of waste polyethylene, waste poly-1-butene, and waste polypropylene; The dosage of the dispersant is 0.1%-0.2%; The dispersant is an anionic dispersant and a nonionic dispersant; The mass ratio of the polyolefin to acrylic acid, methacrylic acid or methyl methacrylate is 1: (0.01-0.02); The solid content of the polyolefin microsphere emulsion is 10-40%.

2. The method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization according to claim 1, characterized in that: The anionic dispersant is an alkyl sulfonate or an alkyl sulfate; the nonionic dispersant is polyethylene oxide, polyoxypropylene ether or polyol fatty acid ester.

3. The method for preparing polyolefin microspheres based on thermal degradation and free radical polymerization according to claim 1, characterized in that: Add polyolefin powder into a pressure reactor with an internal temperature of 120-200°C, a stirring speed of 300-1500 r / min, and a stirring time of 1-4 h.

4. The micro-nano polyolefin microsphere emulsion obtained by the preparation method according to claim 1.

5. Use of the polyolefin microsphere emulsion according to claim 4 in preparing a lithium battery coating diaphragm.

Citation Information

Patent Citations

  • A method for preparing and applying a polyolefin microsphere emulsion with low dispersant content.

    CN115926195B

  • Couple method of polyolefin molecular chain

    CN101450982A

  • Preparation method and application of polyolefin microsphere emulsion with low dispersant content

    CN115926195A

  • Polar polyolefin microsphere as well as preparation method and application thereof

    CN116854952A

  • Recycled polyolefin resin composition and method for producing the same

    JP2010159322A