Preparation method and application of flexible membrane for precise manipulation of liquid by regulating charge distribution

By combining a flexible membrane with a friction rod, the problems of complex electrode arrays and insufficient sustainability in liquid manipulation are solved, achieving efficient, precise and sustainable liquid control, which is suitable for microfluidic chips and chemical analysis.

CN117603490BActive Publication Date: 2024-11-05DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311612645.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-05
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing technologies for liquid manipulation require complex electrode arrays and circuit control, and the sustainability of liquid manipulation is insufficient, with complex pre-processing for charge regulation.

Method used

By combining a flexible membrane with a friction rod, liquids can be precisely controlled by regulating the charge distribution. The flexible membrane is formed by a polymer monomer solution on the substrate surface to create a porous structure. Combined with additive treatment, non-contact liquid control and charge replenishment can be achieved.

Benefits of technology

It enables reusable, programmable liquid manipulation, avoids oil loss, expands the range of applications, is low in cost, simple to operate, suitable for large-scale preparation, and achieves efficient, precise and sustainable liquid control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117603490B_ABST
    Figure CN117603490B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a flexible membrane for precisely controlling a liquid by regulating charge distribution and its application, and relates to the field of microfluidic technology; after cleaning the surface of a substrate, drying it for standby use; adding a polymer monomer to xylene to obtain a polymer monomer solution; pouring the polymer monomer solution on the surface of the cleaned substrate, cooling it to 15-30°C for crystallization, and obtaining a membrane with a porous structure; placing the membrane with a porous structure in an auxiliary agent and soaking it for 15-45 minutes, taking it out and placing it on an inclined plane, and standing it for 5-10 minutes to obtain a target product flexible membrane. The present invention adopts the above steps, and uses the prepared flexible membrane and a friction rod to cooperate to achieve continuous and stable liquid regulation. Even if the initial charge distribution on the surface is uneven, efficient, precise and sustainable liquid movement behavior, including control of transport and segmentation, can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of microfluidics, and in particular to a method for preparing a flexible membrane for precisely controlling liquid by regulating charge distribution and its application. Background Art

[0002] Controllable liquid transport is a basic technology required in the fields of microfluidics, water collection, condensation heat exchange, 3D printing, etc., and is widely used in aerospace, nuclear power energy, biomedicine and other fields. Common electrowetting can manipulate liquids with high precision and flexibility, but it usually requires complex electrode arrays and circuit control. Recently, researchers have proposed a method to manipulate liquids through triboelectrowetting, but it is necessary to ensure uniform surface charge distribution by removing static electricity and high-voltage charging. The preparatory work is relatively complicated, and after use, static electricity must be removed or high-voltage charging must be performed again before it can work again. The sustainability of liquid manipulation is insufficient. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a flexible membrane for precisely controlling liquid by regulating charge distribution and its application, so as to solve the problems of complex and unsustainable limitations of the preparatory work for charge droplet regulation.

[0004] To achieve the above object, the present invention provides a method for preparing a flexible membrane for precisely controlling a liquid by regulating charge distribution, the steps of which are as follows:

[0005] S1, using acetone, deionized water and anhydrous ethanol to clean the surface of the substrate in sequence, and drying it for later use after cleaning;

[0006] S2, adding the polymer monomer into xylene, stirring at 135-155° C. for 1-1.5 hours to obtain a polymer monomer solution;

[0007] S3, pouring the polymer monomer solution in S2 onto the surface of the substrate cleaned in S1, cooling to 15-30° C. for crystallization, and obtaining a membrane with a porous structure;

[0008] S4. Soak the membrane with a porous structure in S3 in an auxiliary agent for 15-45 minutes, take it out and place it on an inclined plane with an inclination of 20-40 degrees, and let it stand for 5-10 minutes to obtain a flexible membrane of the target product.

[0009] Preferably, in S1, the substrate is a plate or coil having strong electronegativity;

[0010] The substrate is one or more of polytetrafluoroethylene, polyvinylidene fluoride, polychlorotrifluoroethylene, polyvinyl fluoride, and polyperfluoroethylene propylene.

[0011] Preferably, in S2, the polymer monomer is one or more of polypropylene, polycarbonate, polyoxymethylene, polyethylene, polyphenylene ether and polyvinyl chloride.

[0012] Preferably, in S4, the auxiliary agent is one or more of silicone oil with a viscosity of 10 to 100 cps, dimethyl silicone oil, glycerin, liquid paraffin, n-butyl stearate, benzyl silicone oil, and ethylmethyl silicone oil.

[0013] The flexible film prepared by the above preparation method.

[0014] Application of the above-mentioned flexible membrane: The flexible membrane is used in microfluidic chips and chemical analysis. When used, the flexible membrane is used in combination with a friction rod to achieve liquid regulation.

[0015] Preferably, insulating material is wound around the metal rod that has been cleaned with acetone, deionized water and anhydrous ethanol in sequence, and the friction rod is obtained after being tightly wrapped with insulating tape.

[0016] Preferably, the insulating material is one or more of nitrile rubber, chloroprene rubber, ethylene propylene rubber, isoprene rubber, silicone rubber, styrene butadiene rubber, and butadiene rubber.

[0017] Preferably, the metal rod is made of one or more of copper, iron, silver, carbon, platinum and gold.

[0018] Therefore, the present invention adopts the above steps to accurately control the charge distribution of the flexible membrane preparation method and application of the liquid, and its beneficial effects are:

[0019] 1. The flexible membrane based on asymmetric charge-controlled droplets prepared by the present invention can effectively avoid oil loss, has good flexibility, and expands the scope of application;

[0020] 2. The friction rod prepared by the present invention continuously replenishes the charge while controlling the liquid in a non-contact manner, so that its surface is always in a fully charged state. It is a reusable and programmable triboelectric control platform;

[0021] 3. The materials used in the present invention are all industrial-grade materials, which are easy to obtain and low in cost. The preparation method used is the drop coating method, which has a simple and easy operation process and can be prepared on a large scale and in large quantities;

[0022] 4. The present invention utilizes a flexible membrane and a friction rod to work together to achieve sustainable and stable liquid regulation. Even if the initial charge distribution on the surface is uneven, efficient, precise and sustainable liquid manipulation can be achieved.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a combined diagram of the surface morphology structure of the membrane with a porous structure and the contact angle of a water drop thereon in the method for preparing the flexible membrane S3 of the present invention;

[0025] Figure 2 is a surface morphology structure diagram of the flexible film obtained in the method for preparing the flexible film S4 of the present invention;

[0026] Figure 3 is a graph showing the relationship between the surface voltage and position of the flexible membrane in Example 1;

[0027] Figure 4 is a side view of 10 μL of deionized water moving linearly on the flexible membrane in Example 1;

[0028] Figure 5 is a diagram of 10 μL of deionized water moving along a “U” trajectory on the flexible membrane in Example 1;

[0029] Figure 6 is a splitting diagram of 10 μL of deionized water on the flexible membrane of Example 1;

[0030] Figure 7 3 is a graph showing the relationship between the surface voltage of the flexible film and the number of frictions in Example 1. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0032] The present invention can be explained in more detail by the following examples. The purpose of disclosing the present invention is to protect all changes and improvements within the scope of the present invention. The present invention is not limited to the following examples.

[0033] Example 1

[0034] S1, using acetone, deionized water and anhydrous ethanol to clean the surface of the substrate in sequence, and drying it for later use after cleaning;

[0035] The substrate is 240mm x 80mm x 2mm PTFE.

[0036] S2, add 5 g of polypropylene into 50 mL of xylene, stir at 135° C. for 1 h to obtain a polypropylene solution;

[0037] S3, pour the polypropylene solution in S2 onto the surface of the cleaned polytetrafluoroethylene in S1, and cool to 20°C for crystallization. As the temperature of the polypropylene solution decreases, the polypropylene begins to nucleate, connects into chains in the polypropylene solution, and aggregates into an interconnected porous structure through phase separation. Combining the porous structure and low surface tension of polypropylene, a porous membrane with a water contact angle of 152° is obtained, such as Figure 1 As shown, the porous structure of the membrane has superhydrophobic properties.

[0038] S4, the membrane with a porous structure in S3 is immersed in silicone oil for 30 minutes, the silicone oil enters the porous structure of the membrane with a porous structure, and then taken out and placed on an inclined plane with an inclination of 30°, and the target product flexible membrane is obtained after standing for 10 minutes, such as Figure 2 shown.

[0039] A friction rod was obtained by winding 0.8 mm nitrile rubber around a metal rod that had been washed with acetone, deionized water and anhydrous ethanol in sequence and wrapping it tightly with an insulating tape.

[0040] The metal rod is a copper rod with a diameter of 8 mm.

[0041] The flexible membrane obtained in this embodiment is applied to microfluidic chips and chemical analysis. The flexible membrane is used in combination with a friction rod to achieve a series of continuous and precise controls on droplets.

[0042] Example 2

[0043] S1, using acetone, deionized water and anhydrous ethanol to clean the surface of the substrate in sequence, and drying it for later use after cleaning;

[0044] The substrate is 100mm x 40mm x 1mm polyvinylidene fluoride;

[0045] S2, add 5 g of polypropylene into 50 mL of xylene, stir at 145° C. for 1.5 h to obtain a polypropylene solution;

[0046] S3. Pour the polypropylene solution in S2 onto the surface of the cleaned polyvinylidene fluoride in S1 and cool it to 20°C for crystallization. As the temperature of the polypropylene solution decreases, the polypropylene begins to nucleate and connect into necklace-like chains in the polypropylene solution. The chains are then aggregated into an interconnected porous structure through phase separation. Combined with the porous structure and low surface tension of the polypropylene, a membrane with a porous structure is obtained.

[0047] S4. Soak the membrane with a porous structure in S3 in silicone oil for 30 minutes. The silicone oil enters the porous structure of the membrane with a porous structure. Take it out and place it on an inclined plane with an inclination of 20°. After standing for 20 minutes, the target product flexible membrane is obtained.

[0048] A friction rod was obtained by winding 0.8 mm nitrile rubber around a metal rod that had been washed with acetone, deionized water and anhydrous ethanol in sequence and wrapping it tightly with an insulating tape.

[0049] The metal rod is a copper rod with a diameter of 6 mm.

[0050] The flexible membrane obtained in this embodiment is applied to microfluidic chips and chemical analysis. The flexible membrane is used in combination with a friction rod to achieve a series of continuous and precise controls on droplets.

[0051] Example 3

[0052] S1, using acetone, deionized water and anhydrous ethanol to clean the surface of the substrate in sequence, and drying it for later use after cleaning;

[0053] The substrate is 200mm x 40mm x 0.8mm polyvinylidene fluoride;

[0054] S2, add 5 g of polypropylene into 50 mL of xylene, stir at 140° C. for 1.5 h to obtain a polypropylene solution;

[0055] S3. Pour the polypropylene solution in S2 onto the surface of the cleaned polyvinylidene fluoride in S1 and cool it to 20°C for crystallization. As the temperature of the polypropylene solution decreases, the polypropylene begins to nucleate and connect into necklace-like chains in the polypropylene solution. The chains are then aggregated into an interconnected porous structure through phase separation. Combined with the porous structure and low surface tension of the polypropylene, a membrane with a porous structure is obtained.

[0056] S4. Soak the membrane with a porous structure in S3 in silicone oil for 30 minutes. The silicone oil enters the porous structure of the membrane with a porous structure. Take it out and place it on an inclined plane with an inclination of 30°. After standing for 10 minutes, the target product flexible membrane is obtained.

[0057] A friction rod was obtained by winding 0.8 mm nitrile rubber around a metal rod that had been washed with acetone, deionized water and anhydrous ethanol in sequence and wrapping it tightly with an insulating tape.

[0058] The metal rod is an iron rod with a diameter of 8 mm.

[0059] The flexible membrane obtained in this embodiment is applied to microfluidic chips and chemical analysis. The flexible membrane is used in combination with a friction rod to achieve a series of continuous and precise controls on droplets.

[0060] Example 4

[0061] a. Use an electrometer to measure the surface voltage of the friction rod in Example 1, taking the position of the friction rod as the origin. The results are as follows: Figure 3 As shown, the surface voltage in the straight line direction is distributed in a gradient shape.

[0062] b. Verify the feasibility of droplet manipulation under uniform and non-uniform surface charge distribution

[0063] In the case of uniform and non-uniform surface charge distribution, a drop of 10 μL of deionized water was dropped on the flexible membrane of Example 1 using a pipette, and a friction rod was placed on a motion table to manipulate the 10 μL deionized water to move linearly. The friction rod was used to change the surface charge distribution to manipulate the movement of the deionized water, such as Figure 4 shown.

[0064] When the friction rod moves along the "U" trajectory, the deionized water can also move along the same trajectory, such as Figure 5 As shown, precise control can be achieved by repeating the process thirty times.

[0065] c. Verify the feasibility of droplet splitting on the prepared flexible membrane

[0066] A 10 μL drop of deionized water was placed on the flexible membrane of Example 1 using a pipette, and the segmentation effect was achieved by adjusting the charge of the deionized water itself and the surface charge gradient. Figure 6 As shown, the deionized water is split into two droplets.

[0067] d. Verify the repeatability of regulation and the absence of post-processing

[0068] After 10 μL of deionized water was manipulated to move along the estimated trajectory on the surface of the flexible membrane in Example 1, the deionized water was absorbed by a paper towel, and then 10 μL of deionized water was dripped into the surface. The operation was repeated 50 times, and the surface voltage of the flexible membrane in Example 1 was measured and analyzed. Figure 7 As shown, it can be seen that after 50 friction operations, the surface voltage has almost no loss and can be precisely controlled without the need for post-processing operations such as deionized air to blow away the charge or high-voltage charging.

[0069] e. Verify the stability of the oil film on the flexible membrane surface

[0070] The flexible membrane in Example 1 was left standing in the air for 7 days, and a drop of 10 μL of deionized water was dropped on the surface of the flexible membrane with a pipette. The movement trajectory of the deionized water could still be precisely controlled, indicating that the additive was not lost after a long period of standing, and the oil film on its surface had strong stability.

[0071] f. Verify the flexibility of the flexible film

[0072] The flexible film in Example 1 was bent 180°, and the flexible film was not broken or cracked. The flexible film in Example 1 was twisted several times, and the flexible film was not broken or cracked. Then the force was released, and it was found that the flexible film in Example 1 could return to its original state without any change.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a flexible membrane for precisely controlling liquid by regulating charge distribution, characterized in that: Here are the steps: S1, using acetone, deionized water and anhydrous ethanol to clean the surface of the substrate in sequence, and drying it for later use after cleaning; S2, adding the polymer monomer into xylene, stirring at 135-155° C. for 1-1.5 hours to obtain a polymer monomer solution; S3, pouring the polymer monomer solution in S2 onto the surface of the substrate cleaned in S1, cooling to 15-30° C. for crystallization, and obtaining a membrane with a porous structure; S4, soaking the membrane with a porous structure in S3 in an auxiliary agent for 15-45 minutes, taking it out and placing it on an inclined plane with an inclination of 20-40 degrees, and letting it stand for 5-10 minutes to obtain a flexible membrane of the target product; The flexible membrane is applied to microfluidic chips and chemical analysis, and the flexible membrane is used in combination with a friction rod to achieve liquid regulation; The segmentation effect is achieved by regulating the charge size of deionized water itself and the surface charge gradient; An insulating material is wound around a metal rod that has been cleaned with acetone, deionized water and anhydrous ethanol in sequence, and the friction rod is tightly wrapped with an insulating tape. The insulating material is one or more of nitrile rubber, chloroprene rubber, ethylene propylene rubber, isoprene rubber, silicone rubber, styrene butadiene rubber and cis-butadiene rubber. The material of the metal rod is one or more of copper, iron, silver, platinum and gold.

2. The method for preparing a flexible membrane for precisely controlling liquid by regulating charge distribution according to claim 1, characterized in that: In S1, the substrate is a sheet or coil with strong electronegativity; The substrate is one or more of polytetrafluoroethylene, polyvinylidene fluoride, polychlorotrifluoroethylene, polyvinyl fluoride, and polyperfluoroethylene propylene.

3. The method for preparing a flexible membrane for precisely controlling liquid by regulating charge distribution according to claim 1, characterized in that: In S4, the auxiliary agent is one or more of dimethyl silicone oil with a viscosity of 10 to 100 cps, glycerin, liquid paraffin, n-butyl stearate, benzyl silicone oil, and ethylmethyl silicone oil.

4. The flexible film prepared according to the preparation method according to any one of claims 1 to 3.