A waterproof construction method for sealing seams of doors and windows

By filling the gap between window frames or door frames with the installation holes, the hydrolysis reaction between rice husk ash and expanded vitrified microbeads is used to form a silicon sol connection, which solves the problems of water seepage and backflow in the existing technology, and achieves efficient sealing and Improved structural strength.

CN117605378BActive Publication Date: 2024-11-22NEW WANGJI TECH ENG GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311574965.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-23
Publication Date
2024-11-22
Estimated Expiration
2043-11-23

AI Technical Summary

Technical Problem

In the prior art, there are problems of water seepage and backflow at the connection between window frames or door frames and building exterior walls, and the flexible foam glue used has poor anti-aging effect and is prone to glue opening and breaking.

Method used

Modified concrete is used to fill the gap between the window frame or door frame and the installation hole. The modified concrete is composed of sulfaluminate cement, fine aggregate, coarse aggregate, rice husk ash and expanded vitrified microbeads, and is formed by hydrolysis reaction. Silicone sol connection achieves rapid coagulation and multi-stage filling, enhancing structural strength.

Benefits of technology

Good sealing, waterproofing and thermal insulation are achieved, problems such as water leakage, fracture and fall off are avoided, and structural strength and construction efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FHA0000007682020000011
    Figure FHA0000007682020000011
  • Figure GHA0000007682030000021
    Figure GHA0000007682030000021
  • Figure GHA0000007682030000091
    Figure GHA0000007682030000091
Patent Text Reader

Abstract

The invention discloses a waterproof construction method for sealing seams of doors and windows, comprising the following steps: S1, fixing a window frame or a door frame to the installation hole after roughening both sides and an upper opening of an installation hole on an external wall; S2, filling a gap between the window frame or the door frame and the installation hole with modified concrete; during the construction process of the modified concrete, silanol groups and hydroxyl groups on the surface of silica sol ions form a connection between rice husk ash and expanded vitrified microspheres through hydrogen bonds; S3, the modified concrete solidifies and hardens, and is cured to complete the waterproof construction of the window frame or the door frame; the invention uses concrete to fill the gap between the window frame or the door frame and the installation hole, and uses multi-level structural materials in the concrete to achieve multi-level filling of space during solidification and curing, and has good structural strength and rapid solidification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building structures, and in particular to a waterproof construction method for sealing seams of doors and windows. Background Art

[0002] The window frame or door frame is a transition structure between the wall and the window or door, which plays a role in fixing and preventing the surrounding walls from collapsing. The construction quality of the window frame on the exterior wall of the building is a very intuitive and sensitive indicator for residents to judge the quality of the building. In the prior art, the connection between the window frame or door frame and the exterior wall of the building is mostly sealed with cement mortar, and the technical problems are water seepage and backflow. In the prior art, there is also a construction scheme using foam glue for sealing, such as the invention patent CN115126381A, which records that the foaming agent should be applied continuously, and the part with a width exceeding the width of the window frame should be pressed into the inside of the window frame before the foaming agent condenses. The foaming agent structure is required to be complete, and the width is the same as the frame window or slightly smaller than the window frame width. However, in the actual construction process, the foaming glue is a flexible material, and the anti-aging effect is poor, and there are problems of debonding and breaking. Summary of the invention

[0003] The purpose of the present invention is to provide a waterproof construction method for sealing the gaps of doors and windows. The present invention uses concrete to fill the gaps between the window frame or door frame and the installation opening, and uses the multi-level structural materials in the concrete to achieve multi-level filling of the space during the solidification process. The method has good structural strength and rapid solidification.

[0004] To solve this technical problem, the technical solution of the present invention is: a window frame or door frame and a waterproof construction method for sealing the seams of doors and windows, comprising the following steps:

[0005] S1. Use high-strength mortar to roughen the two sides and the top of the installation hole on the exterior wall, and then use expansion bolts to fix the window frame or door frame to the installation hole;

[0006] S2, filling the gap between the window frame or door frame and the installation opening with modified concrete;

[0007] The modified concrete comprises the following components: sulphoaluminate cement, fine aggregate, coarse aggregate, rice husk ash with loose structure, polycarboxylic acid early strength water reducing agent, expanded vitrified microspheres and water;

[0008] During the construction of modified concrete, the silicon dioxide on the surface of the loose rice husk ash and the silicon dioxide on the surface of the expanded vitrified microspheres are hydrolyzed to form silica sol ions, and the silanol groups (-SiOH) and hydroxyl groups (-OH) on the surface of the silica sol ions form a connection between the rice husk ash and the expanded vitrified microspheres through hydrogen bonds.

[0009] S3. The modified concrete solidifies and hardens, and then is cured to complete the waterproofing construction of the window frame or door frame.

[0010] Preferably, the modified concrete slurry comprises the following substances in parts by mass:

[0011]

[0012] Preferably, the mixing method of the modified concrete comprises the following steps:

[0013] S21, stirring and dispersing the expanded vitrified microspheres and the rice husk ash having a loose structure evenly;

[0014] S22, adding an aqueous solution with a pH value of 8 to 9 to the S21 material, stirring and heating, wherein the silicon dioxide particles in the rice husk ash are hydrolyzed to form silica sol particles, and the silicon dioxide on the surface of the expanded vitrified microspheres is hydrolyzed to form silica sol particles, and during the stirring process, the rice husk ash and the expanded vitrified microspheres are connected by hydrogen bonds through the silanol groups (-SiOH) and hydroxyl groups (-OH) of the silica sol particles;

[0015] S23, adding the remaining components to the material after S22 according to the mass fractions, replenishing water to the mass fraction of water in the modified concrete composition, stirring evenly, and obtaining modified concrete slurry.

[0016] Preferably, the heating temperature in S22 is 50°C to 60°C, and the stirring time is 6 hours to 9 hours. The present invention utilizes long-term stirring under alkaline conditions to promote the hydrolysis of silicon dioxide particles in rice husk ash and the hydrolysis of silicon dioxide on the surface of expanded vitrified microspheres, and the two further realize the connection between the two substances by forming silica sol during the hydrolysis process. On the one hand, the expanded vitrified microspheres surrounded by rice husk ash form a good and reliable interface contact through the hydration of silica sol and cement. On the other hand, the multi-void structure caused by the presence of plant sources in the rice husk ash uniformly dispersed in the concrete, the thermal expansion and contraction of the cured waterproof concrete when the temperature changes greatly occurs due to the porous structure of the rice husk ash in its own structure, which causes internal buffering, thereby effectively suppressing the volume change caused by water loss or temperature change, and forming a tight connection with the front wall window frame or door frame, thereby ensuring good sealing, waterproof and thermal insulation.

[0017] Preferably, the method for preparing rice husk ash comprises the following steps:

[0018] A1. Dried rice husk powder;

[0019] A2. Constant temperature combustion of the rice husk obtained in A1. The combustion process conditions are as follows:

[0020] 800°C to 900°C, 1 hour to 1.5 hours;

[0021] Cooling to obtain rice husk ash;

[0022] The rice husk ash includes activated carbon having a pore structure obtained by removing organic matter and silicon dioxide grown on the activated carbon;

[0023] A3, using hydrochloric acid solution to soak and activate the rice husk ash obtained in A2 to remove metal oxides.

[0024] The rice husk powder in A1 is preferably sieved through a 200-270 mesh sieve. The rice husk powder used in the present invention has relatively small particles and is suitable for multi-stage filling with coarse aggregate, fine aggregate, expanded vitrified microspheres surrounded by rice husk ash, and sulphoaluminate cement in concrete to obtain a stable window frame or door frame waterproof construction structure.

[0025] The process conditions for hydrochloric acid activation of rice husk ash in A3 are preferably as follows:

[0026] Rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:(2 to 3), heated to 80 to 100° C., stirred for 2 to 3 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

[0027] Preferably, during the setting and hardening process of the S3 modified concrete, the silica sol of rice husk ash and the silica sol of expanded vitrified microspheres participate in the hydration of cement, and the rice husk ash surrounds the expanded vitrified microspheres. The rice husk ash and the expanded vitrified microspheres are connected by chemical bonds, and the volume of the composite is increased by the compound of the rice husk ash and the expanded vitrified microspheres, so that the steric hindrance of the rice husk ash and the expanded vitrified microspheres is used to form a step-by-step filling in the process of mixing and construction, so as to avoid uneven dispersion of small particles such as rice husk ash and expanded vitrified microspheres in the concrete reduction, and the obtained waterproof construction structure has an uneven concrete structure after curing, especially between the window frame or door frame and the window opening wall that need to be constructed in the vertical direction, which is greatly affected by gravity. Once the moisture in the concrete is easily gathered by gravity, it will cause the moisture of the concrete slurry at a higher position in the vertical direction to migrate to a lower position, further resulting in inconsistent structural strength of the vertical waterproof construction structure concrete in the vertical direction, and insufficient cement hydration reaction, resulting in insufficient structural strength, and it is difficult to ensure waterproofness. In the present invention, silica sol is used to promote water dispersion, and the adsorption effect of porous carbon is further coordinated to achieve water buffering. As the hydration proceeds, the porous carbon continuously releases the water therein to prevent the water from gathering and flowing downwards. At the same time, due to the slow release of water in the porous carbon in the concrete, the concrete sets quickly in the early stage, sets quickly, and has a smooth filling effect.

[0028] By adopting the above technical solution, the beneficial effects of the present invention are:

[0029] The present invention utilizes the coarse aggregate, fine aggregate, expanded vitrified microspheres and sulphoaluminate cement to disperse and move relative positions during the mixing and pouring of concrete, forming a spontaneous graded filling to form a stable structure; the loose rice husk has a certain water storage capacity, and forms a stable filling structure support with the coarse aggregate, fine aggregate and expanded vitrified microspheres, and solidifies quickly; at the same time, the loose rice husk has a certain water storage process, and the stored water is continuously released under the driving force of the concentration gradient change as the hydration reaction of cement in the concrete proceeds, on the one hand, it avoids the slow coagulation speed in the concrete slurry constructed in the vertical direction, and the water in the concrete slurry is separated from other components under the action of gravity; it also avoids the hydration of cement causing the concrete to have a non-dense and unstable structure after solidification due to lack of water or excessive water; therefore, the waterproof construction method for window frames or door frames proposed by the present invention can obtain good structural strength, and can improve the traditional existing problems such as leakage, breakage, and falling off to a certain extent. DETAILED DESCRIPTION

[0030] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0031] Example 1

[0032] This embodiment discloses a waterproof construction method for a window frame or a door frame applied to a door or window caulking, comprising the following steps:

[0033] S1. Use high-strength mortar to roughen the two sides and the top of the installation hole on the exterior wall, and then use expansion bolts to fix the window frame or door frame to the installation hole;

[0034] S2, filling the gap between the window frame or door frame and the installation opening with modified concrete;

[0035] The modified concrete comprises the following components: sulphoaluminate cement, fine aggregate, coarse aggregate, rice husk ash with loose structure, polycarboxylic acid early strength water reducing agent, expanded vitrified microspheres and water;

[0036] During the construction of modified concrete, the loose rice husk ash structure forms silica sol ions through the hydrolysis of silica on the surface and the silica on the surface of expanded vitrified microspheres coated with silica sol. The silanol groups (-SiOH) and hydroxyl groups (-OH) on the surface of the silica sol ions form a connection between the rice husk ash and the expanded vitrified microspheres through hydrogen bonds.

[0037] S3. The modified concrete solidifies and hardens, and then is cured to complete the waterproofing construction of the window frame or door frame.

[0038] The modified concrete slurry described in this embodiment is shown in Table 1 according to the mass percentage.

[0039] The mixing method of the modified concrete described in this embodiment comprises the following steps:

[0040] S21, stirring and dispersing the expanded vitrified microspheres and the rice husk ash having a loose structure evenly;

[0041] S22, adding KOH aqueous solution with a pH value of 8 to the material S21, stirring and heating, wherein the silicon dioxide particles in the rice husk ash are hydrolyzed to form silica sol particles, and the silicon dioxide on the surface of the expanded vitrified microspheres is hydrolyzed to form silica sol particles, and during the stirring process, the rice husk ash and the expanded vitrified microspheres are connected by hydrogen bonds through the silanol group (-SiOH) and hydroxyl group (-OH) of the silica sol particles;

[0042] In S22, the heating temperature is 50°C and the stirring time is 6 hours.

[0043] S23, adding the remaining components to the material after S22 according to the mass fractions, replenishing water to the mass fraction of water in the modified concrete composition, stirring evenly, and obtaining modified concrete slurry.

[0044] The present invention utilizes long-term stirring under alkaline conditions to promote the hydrolysis of silicon dioxide particles in rice husk ash and the hydrolysis of silicon dioxide on the surface of expanded vitrified microspheres, and the two further achieve connection between the two substances by forming silica sol during the hydrolysis process. The expanded vitrified microspheres surrounded by rice husk ash form a good and reliable interface contact through the hydration of silica sol and cement on the one hand, and on the other hand, the rice husk ash is evenly dispersed in the concrete. Due to the multi-porous structure of plant origin, the thermal expansion and contraction of the cured waterproof concrete when the temperature changes greatly is internally buffered due to the porous structure of the rice husk ash in its own structure, thereby effectively suppressing the volume change caused by water loss or temperature change, and forming a tight connection with the front wall window frame or door frame, thereby ensuring good sealing, waterproof and thermal insulation properties.

[0045] The method for preparing rice husk ash described in this embodiment comprises the following steps:

[0046] A1. Dried rice husk powder;

[0047] A2. Constant temperature combustion of the rice husk obtained in A1. The combustion process conditions are as follows:

[0048] 800°C, 1.5 hours;

[0049] Cooling to obtain rice husk ash;

[0050] The rice husk ash includes activated carbon having a pore structure obtained by removing organic matter and silicon dioxide grown on the activated carbon;

[0051] A3, using hydrochloric acid solution to soak and activate the rice husk ash obtained in A2 to remove metal oxides.

[0052] In this embodiment, the rice husk powder in A1 is sieved through a 200-mesh sieve. The rice husk powder used in the present invention has relatively small particles and is suitable for multi-stage filling with coarse aggregate, fine aggregate, expanded vitrified microspheres surrounded by rice husk ash, and sulphoaluminate cement in concrete to obtain a stable window frame or door frame waterproof construction structure.

[0053] The process conditions for hydrochloric acid activation of rice husk ash in A3 in this embodiment are as follows:

[0054] Rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:2, heated to 80°C, stirred for 2 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

[0055] In the present embodiment, during the solidification and hardening process of the S3 modified concrete, the silica sol of rice husk ash and the silica sol of expanded vitrified microspheres participate in the hydration of cement, and the rice husk ash surrounds the expanded vitrified microspheres.

[0056] Example 2

[0057] The main difference between this embodiment and embodiment 1 is the composition of the modified concrete slurry, as shown in Table 1;

[0058] The differences between the preparation process parameters of this embodiment and embodiment 1 are as follows:

[0059] S22, adding KOH aqueous solution with a pH value of 9 to the material S21, stirring and heating;

[0060] In S22, the heating temperature is 60°C and the stirring time is 7 hours.

[0061] In the preparation method of rice husk ash described in this embodiment, the combustion process conditions in step A2 are as follows:

[0062] 850°C, 1.5 hours;

[0063] In this embodiment, the rice husk powder in A1 is sieved through a 270-mesh sieve.

[0064] The process conditions for hydrochloric acid activation of rice husk ash in A3 in this embodiment are as follows:

[0065] Rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:2, heated to 90° C., stirred for 3 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

[0066] Example 3

[0067] The main difference between this embodiment and embodiment 1 is the composition of the modified concrete slurry, as shown in Table 1;

[0068] The differences between the preparation process parameters of this embodiment and embodiment 1 are as follows:

[0069] S22, adding KOH aqueous solution with a pH value of 8 to the material S21, stirring and heating;

[0070] In S22, the heating temperature is 55°C and the stirring time is 8 hours.

[0071] The process conditions for combustion in step A2 of the method for preparing rice husk ash described in this embodiment are as follows:

[0072] 900°C, 1.0 hour;

[0073] In this embodiment, the rice husk powder in A1 was sieved through a 200-mesh sieve.

[0074] The process conditions for hydrochloric acid activation of rice husk ash in A3 in this embodiment are as follows:

[0075] The rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:3, heated to 100° C., stirred for 2 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

[0076] Example 4

[0077] The main difference between this embodiment and embodiment 1 is the composition of the modified concrete slurry, as shown in Table 1;

[0078] The differences between the preparation process parameters of this embodiment and embodiment 1 are as follows:

[0079] S22, adding KOH aqueous solution with a pH value of 9 to the material S21, stirring and heating;

[0080] In S22, the heating temperature is 60°C and the stirring time is 9 hours.

[0081] The process conditions for combustion in step A2 of the method for preparing rice husk ash described in this embodiment are as follows:

[0082] 850°C, 1.0 hour;

[0083] In this embodiment, the rice husk powder in A1 is sieved through a 270-mesh sieve.

[0084] The process conditions for hydrochloric acid activation of rice husk ash in A3 in this embodiment are as follows:

[0085] Rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:3, heated to 90° C., stirred for 3 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

[0086] Comparative Example

[0087] This comparative example discloses a waterproof construction method for a window frame or a door frame applied to the sealing of doors and windows, comprising the following steps:

[0088] S1. Use high-strength mortar to roughen the two sides and the top of the installation hole on the exterior wall, and then use expansion bolts to fix the window frame or door frame to the installation hole;

[0089] S2, filling the gap between the window frame or door frame and the installation opening with modified concrete;

[0090] The modified concrete comprises the following components: sulphoaluminate cement, fine aggregate, coarse aggregate, rice husk ash with loose structure, polycarboxylic acid early strength water reducing agent, expanded vitrified microspheres and water; the amount of each component in this comparative example is the same as that in Example 4. The modified concrete in this comparative example is directly mixed and stirred to obtain a modified concrete slurry;

[0091] S3. The modified concrete solidifies and hardens, and then is cured to complete the waterproofing construction of the window frame or door frame.

[0092] The method for processing rice husk and rice husk ash in this comparative example is the same as that in Example 4.

[0093] Table 1 Composition of concrete slurries obtained in Examples 1 to 4 (parts by mass)

[0094]

[0095]

[0096] The concrete obtained in Examples 1 to 4 and the comparative example was filled in a long trough structure with a length of 1500 mm, a width of 30 mm, and a thickness of 60 mm to simulate the situation of installing the waterproof construction of the window frame or door frame in the vertical gap of the installation hole. The filled concrete slurry was allowed to stand at room temperature until initial setting, and then the long trough structure was placed vertically. Different height positions of 28D were tested, and the heights of 250 mm, 750 mm, and 1250 mm from the lower end were respectively measured as positions A, B, and C, and their compressive strength was tested. The specific data are shown in Table 2. The drying shrinkage rate of the obtained concrete for 60 days was also tested, as shown in Table 2 for details.

[0097] Table 2 Compressive strength of concrete at different heights obtained in Examples 1 to 4 and Comparative Examples

[0098] project A position B position C position Drying shrinkage Example 1 127.8MPa 126.2MPa 126.1MPa 289με Example 2 127.8MPa 126.9MPa 127.4MPa 287με Example 3 131.6MPa 130.4MPa 130.7MPa 272με Example 4 132.6MPa 131.0MPa 130.2MPa 267με Comparative Example 80.5MPa 75.2MPa 68.9MPa 316με

[0099] The thermal conductivity and water absorption of the waterproof concrete were further tested. The specific data are shown in Table 3.

[0100] Table 3 Thermal conductivity and water absorption of modified concrete obtained in Examples 1 to 4 and Comparative Example

[0101]

[0102]

[0103] Combining Table 3 and Table 4, it can be seen that rice husk ash and expanded vitrified microspheres are connected by chemical bonds, and the volume of the composite is increased by the combination of rice husk ash and expanded vitrified microspheres, so that the space steric hindrance of the rice husk ash and expanded vitrified microspheres is used to form a step-by-step filling in the process of mixing and construction, so as to avoid uneven dispersion of small particles such as rice husk ash and expanded vitrified microspheres in concrete reduction, and the cured concrete structure of the obtained waterproof construction structure is uneven, especially between the window frame or door frame and the window opening wall that need to be constructed in the vertical direction, which is greatly affected by gravity. Once the moisture in the concrete is easily gathered by gravity, it will cause the moisture of the concrete slurry in a higher position in the vertical direction to migrate to a lower position, further resulting in inconsistent structural strength of the vertical waterproof construction structure concrete in the vertical direction, and the hydration reaction of cement is insufficient, resulting in insufficient structural strength, and waterproofness is also difficult to ensure. While using silica sol to promote water dispersion in the present invention, the adsorption effect of porous carbon is further coordinated to achieve water caching. As the hydration proceeds, the porous carbon continuously releases the water therein to prevent the water from gathering and flowing downwards. At the same time, due to the slow release of water in the porous carbon in the concrete, the concrete solidifies quickly in the early stage, sets faster, and has a smooth filling effect.

[0104] In order to ensure that the construction method proposed by the present invention has high efficiency, the vertical space of the installation hole can be filled alternately during construction, or the concrete can be positioned with auxiliary tools to prevent the concrete from flowing before solidification.

Claims

1. A waterproof construction method for sealing the seams of doors and windows. Features: The following steps are involved: S1. Use high-strength mortar to roughen the two sides and the top of the installation hole on the exterior wall, and then use expansion bolts to fix the window frame or door frame to the installation hole; S2, filling the gap between the window frame or door frame and the installation opening with modified concrete; The modified concrete comprises the following components: sulphoaluminate cement, fine aggregate, coarse aggregate, rice husk ash with loose structure, polycarboxylic acid early strength water reducing agent, expanded vitrified microspheres and water; During the construction of modified concrete, the silicon dioxide on the surface of the loose rice husk ash and the silicon dioxide on the surface of the expanded vitrified microspheres are hydrolyzed to form silica sol ions, and the silanol groups and hydroxyl groups on the surface of the silica sol ions form a connection between the rice husk ash and the expanded vitrified microspheres through hydrogen bonds. S3. The modified concrete solidifies and hardens, and then is maintained to complete the waterproofing of the window or door frame; The modified concrete slurry comprises the following substances in parts by mass: The mixing method of the modified concrete comprises the following steps: S21, stirring and dispersing the expanded vitrified microspheres and the rice husk ash having a loose structure evenly; S22, adding an aqueous solution with a pH value of 8 to 9 to the S21 material, stirring and heating, wherein the silicon dioxide particles in the rice husk ash are hydrolyzed to form silica sol particles, and the silicon dioxide on the surface of the expanded vitrified microspheres is hydrolyzed to form silica sol particles, and during the stirring process, the rice husk ash and the expanded vitrified microspheres are connected by hydrogen bonds through the silanol groups and hydroxyl groups of the silica sol particles; S23, adding the remaining components to the material after S22 according to the mass fractions, replenishing water to the mass fraction of water in the modified concrete composition, stirring evenly, and obtaining modified concrete slurry; The method for preparing rice husk ash comprises the following steps: A1. Dried rice husk powder; A2. Constant temperature combustion of the rice husk obtained in A1. The combustion process conditions are as follows: 800°C to 900°C, 1 hour to 1.5 hours; Cooling to obtain rice husk ash; The rice husk ash includes activated carbon having a pore structure obtained by removing organic matter and silicon dioxide grown on the activated carbon; A3, using hydrochloric acid solution to soak and activate the rice husk ash obtained in A2 to remove metal oxides.

2. The construction method according to claim 1, Features: In S22, the heating temperature is 50° C. to 60° C., and the stirring time is 6 hours to 9 hours.

3. The construction method according to claim 1, Features: The rice husk powder in A1 was sieved through a 200-270 mesh sieve.

4. The construction method according to claim 1, Features: The process conditions for hydrochloric acid activation of rice husk ash in A3 are as follows: Rice husk ash is soaked in 16% hydrochloric acid by mass, mixed evenly, the mass ratio of rice husk ash to hydrochloric acid is 1:(2 to 3), heated to 80 to 100° C., stirred for 2 to 3 hours to obtain acid-treated rice husk ash, washed to neutrality, and dried.

5. The construction method according to claim 1, Features: During the setting and hardening process of S3 modified concrete, the silica sol of rice husk ash and the silica sol of expanded vitrified microspheres participate in the hydration of cement, and the rice husk ash surrounds the expanded vitrified microspheres.