Preparation method of low temperature resistant and high rate sodium ion battery negative electrode material

By preparing composite carbon nanotubes and conductive additives, the problem of poor performance of sodium ion battery anode material at low temperatures and high magnifications is solved, and the cyclic stability and electrochemical performance of the material are improved.

CN117658111BActive Publication Date: 2024-11-19ANHUI NANDU HUATUO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311702026.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2024-11-19
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

Existing sodium ion battery anode materials show poor cycle stability and rate performance at low temperatures or high magnifications, which easily lead to material structure failure and capacity attenuation.

Method used

By the preparation method, a combination of pretreatment of carbon nanotubes, activated nanotubes, modified nanotubes and conductive additives, the composite carbon nanotubes are generated by reactions under acidic conditions and calcined under an atmosphere containing acetylene to increase the Electronic conductivity and sodium ion storage sites improve the cyclic stability and electrochemical properties of the material.

Benefits of technology

The cycling stability and electrochemical performance of the negative electrode material of sodium ion battery at low temperature and high magnification is significantly improved, the volume changes caused by the embedding and disengagement of sodium ions are reduced, and the capacity retention rate of the material is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004602322570000111
    Figure BDA0004602322570000111
  • Figure BDA0004602322570000121
    Figure BDA0004602322570000121
Patent Text Reader

Abstract

The present invention discloses a method for preparing a low-temperature resistant and high-rate sodium ion battery negative electrode material, and belongs to the technical field of negative electrode material processing. The present invention is used to solve the technical problem that the prior art sodium ion battery negative electrode material shows good cycle stability and rate performance at low temperature or high rate, and the preparation method of the low-temperature resistant and high-rate sodium ion battery negative electrode material comprises the following steps: adding pretreated carbon nanotubes and activation solution to a three-necked flask and stirring, the temperature of the three-necked flask is increased to 88-92°C at a heating rate of 0.3°C / min, and heat preservation treatment is performed for 2-3h, and post-processing is performed to obtain activated nanotubes. The negative electrode material prepared by the present invention not only shows stable cycle stability performance in a high-rate environment, but also shows good cycle stability, discharge specific capacity retention and first coulomb efficiency in a low-temperature environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of negative electrode material processing, and in particular to a method for preparing a low-temperature resistant and high-rate negative electrode material for a sodium ion battery. Background Art

[0002] With the continuous advancement of science and technology, people's demand for batteries is increasing, especially the requirements for high energy density, long life and stability in extreme environments. As a new type of energy storage system, sodium-ion batteries have the advantages of potential high energy density, low cost and suitability for large-scale energy storage applications. However, the performance of sodium-ion batteries is limited by the negative electrode materials, especially the performance in low temperature environments.

[0003] The existing negative electrode materials for sodium ion batteries, such as hard carbon, soft carbon, and alloys, have reduced conductivity and limited ion transport under low temperature conditions, resulting in reduced energy storage capacity. At high rates, the battery's charge and discharge rates accelerate, which brings greater stress and ion diffusion difficulties to the negative electrode materials, and easily leads to structural damage and capacity decay of the materials. The existing negative electrode materials made of hard carbon or soft carbon materials will change their pore size distribution and specific surface area during rapid charge and discharge, resulting in reduced sodium ion insertion / extraction kinetics, increased brittleness of the negative electrode materials, volume changes, and other problems, leading to material pulverization and fracture. The sodium ion battery negative electrode materials show excellent cycle stability and rate performance at low temperatures or high rates, which need to be further improved.

[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a low-temperature resistant, high-rate sodium ion battery negative electrode material, which is used to solve the technical problem that the sodium ion battery negative electrode material in the prior art exhibits good cycle stability and rate performance at low temperature or high rate and needs to be further improved.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A method for preparing a low-temperature resistant, high-rate sodium ion battery negative electrode material comprises the following steps:

[0008] S1, adding the pretreated carbon nanotubes and the activation solution into a three-necked flask and stirring, raising the temperature of the three-necked flask to 88-92°C at a heating rate of 0.3°C / min, keeping the temperature for 2-3h, and post-treating to obtain activated nanotubes;

[0009] S2, adding activated nanotubes, deionized water, sodium vanadate and titanium tetrachloride into a three-necked flask and stirring, adding hydrochloric acid dropwise into the three-necked flask, raising the temperature of the three-necked flask to 65-75° C., keeping the temperature for reaction for 2-3 hours, and post-treating to obtain modified nanotubes;

[0010] S3, adding the modified nanotubes into an atmosphere furnace loaded with a protective gas atmosphere, raising the temperature of the atmosphere furnace to 600-650°C at a heating rate of 5°C / min, and heat preservation for 4-6 hours, and the atmosphere furnace is naturally cooled to room temperature to obtain composite carbon nanotubes;

[0011] S4. Add the composite nanotubes, acetylene black, conductive additive, binder and N-methylpyrrolidone into a beaker for slurry mixing to obtain a mixed slurry. Evenly apply the mixed slurry to the surface of the carbon fiber cloth, and then perform post-processing to obtain the negative electrode material.

[0012] Furthermore, in step S1, the activation solution is composed of 98wt% sulfuric acid, 65wt% nitric acid, potassium permanganate and hydrogen peroxide in a dosage ratio of 5g:2g:0.3g:4mL, the dosage ratio of the pretreated carbon nanotubes and the activation solution is 1g:7mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is lowered to room temperature, filtered, the filter cake is washed with purified water until neutral, the filter cake is transferred to a drying oven at a temperature of 70-80°C, and dried to constant weight to obtain activated nanotubes.

[0013] Furthermore, the preparation method of pretreated carbon nanotubes is: adding multi-walled carbon nanotubes and iron oxide into an atmosphere furnace at a temperature of 400-450°C, introducing air into the atmosphere furnace at a flow rate of 10mL / min, heat preservation for 60-80min, and post-treatment to obtain pretreated carbon nanotubes.

[0014] Furthermore, the weight ratio of the multi-walled carbon nanotubes to iron oxide is 10:1, and the post-treatment operation includes: after the reaction is completed, the atmosphere furnace temperature is lowered to room temperature, the carbon nanotubes and 5 mol / L hydrochloric acid are added to the flask at a dosage ratio of 1g:8mL and stirred, the temperature of the flask is increased to reflux the system, and the heat treatment is carried out for 3-5h, the temperature of the flask is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80°C and dried to constant weight to obtain pretreated carbon nanotubes.

[0015] Furthermore, in step S2, the dosage ratio of sodium vanadate and titanium tetrachloride is 1 mol:1 mol, the dosage ratio of the activated nanotubes, deionized water, sodium vanadate and hydrochloric acid is 4 g:15 mL:2 g:5 mL, the concentration of the hydrochloric acid is 6-8 mol / L, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is reduced to room temperature, suction filtration, the filter cake is washed with purified water until neutral, the filter cake is transferred to a drying oven at a temperature of 70-80° C., and dried to constant weight to obtain modified nanotubes; in step S3, the protective gas atmosphere is composed of acetylene and nitrogen in a volume ratio of 1:19.

[0016] Further, the conductive additive is processed by the following steps:

[0017] A1. Add cobalt acetate and ethylene glycol into a three-necked flask and stir until the system is dissolved. Add Tween 80 and glucose into the three-necked flask. Raise the temperature of the three-necked flask to 120-130° C., keep warm and stir for 10-12 hours, and post-treat to obtain caramelized glucose.

[0018] A2. Evenly mix caramelized glucose and sulfur powder and add them into an argon-protected atmosphere furnace. The temperature of the atmosphere furnace is raised to 650-690° C. and the mixture is kept warm for 4-6 hours. The conductive additive is obtained by post-processing.

[0019] Furthermore, in step A1, the dosage ratio of cobalt acetate, ethylene glycol, Tween 80 and glucose is 1g:15mL:0.6g:1.5g, and the post-processing operation includes: after the reaction is completed, the temperature of the three-necked flask is reduced to room temperature, the filter is filtered, the filter cake is washed three times with anhydrous ethanol and then dried, the filter cake is transferred to a drying oven at a temperature of 60-70°C, and dried to constant weight to obtain caramelized glucose; in step A2, the weight ratio of caramelized glucose and sulfur powder is 3:1, and the post-processing operation includes: after the reaction is completed, the temperature of the atmosphere furnace is reduced to room temperature, the material is discharged, the calcined powder is washed three times with methanol and then filtered, the filter cake is transferred to a drying oven at a temperature of 55-65°C, and dried to constant weight to obtain a conductive additive.

[0020] Furthermore, in step S4, the weight ratio of the composite nanotubes, acetylene black, conductive additive, binder and N-methylpyrrolidone is 7:2:1:1:4, the binder is polyvinylidene fluoride, and the post-processing operation includes: transferring the carbon fiber cloth coated with the mixed slurry to a drying oven at a temperature of 60-70°C, vacuum drying to constant weight, and using a punching machine to punch out to obtain a negative electrode material with a diameter of 10 mm.

[0021] The present invention has the following beneficial effects:

[0022] The sodium ion battery negative electrode material provided by the present invention is prepared by subjecting multi-walled carbon nanotubes to high-temperature oxidation treatment by means of iron oxide powder, thereby changing the morphology and structure of the multi-walled carbon nanotubes and increasing the roughness of the pretreated carbon nanotubes. After the pretreated carbon nanotubes are treated with an activation solution, a large number of active functional groups such as hydroxyl groups and carboxyl groups are formed on the surface of the activated nanotubes, thereby increasing the polarity and hydrophilicity of the activated nanotubes and making them more likely to interact with sodium vanadate and titanium tetrachloride. The rough surface can also provide more reaction sites, thereby increasing the adsorption performance of the activated nanotubes. Under acidic conditions, sodium vanadate reacts with titanium tetrachloride to generate precipitates that grow in the form of microspheres and attach to the modified nanotubes. High-temperature calcination is performed in a gas atmosphere containing acetylene, and acetylene is decomposed into H2 and C during the calcination process. H2 is easy to form oxygen defects on the nanotube material at high temperature, thereby increasing the electronic conductivity of the nanotube material, while C will be uniformly The conductive additive is uniformly coated on the surface of the particles, promoting the particles and the nanotubes to form a stable whole, which is beneficial to increasing the cycle stability of the nanotube material; after the cobalt acetate is dissolved in the hot ethylene glycol environment, the cobalt acetate and glucose are uniformly dispersed under the action of Tween 80 as a dispersant, and the glucose is decomposed and coked to separate from the ethylene glycol under the action of high temperature, and the cobalt acetate attached to the coked glucose reacts with the sulfur powder under high temperature to generate cobalt sulfide, and the coked glucose generates carbon under high temperature to coat the cobalt sulfide to obtain a conductive additive. Since the conductive additive has high electrochemical activity, it can provide more sodium ion storage sites in a low temperature environment, thereby improving the capacity retention rate of the negative electrode material, and reducing the volume change of the negative electrode material caused by the embedding and extraction of sodium ions in the negative electrode material during the charge and discharge process, thereby improving the cycle performance of the sodium ion negative electrode material, and then improving the electrochemical performance of the sodium ion negative electrode material. DETAILED DESCRIPTION

[0023] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] The method for preparing the low temperature resistant and high rate sodium ion battery negative electrode material provided in this embodiment comprises the following steps:

[0026] S1. Preparation of pretreated carbon nanotubes

[0027] Weigh: 20 g of multi-walled carbon nanotubes and 2 g of nano-iron oxide powder are added to an atmosphere furnace at a temperature of 400°C, and air is introduced into the atmosphere furnace at a flow rate of 10 mL / min. The temperature is kept warm for 60 minutes, and the temperature of the atmosphere furnace is lowered to room temperature. Multi-walled carbon nanotubes and 5 mol / L hydrochloric acid are added to the flask in a dosage ratio of 1g:8mL and stirred. The temperature of the flask is increased to reflux of the system, and the temperature is kept warm for 3 hours. The temperature of the flask is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain pretreated carbon nanotubes.

[0028] S2. Preparation of composite nanotubes

[0029] Add 98wt% sulfuric acid, 65wt% nitric acid, potassium permanganate and hydrogen peroxide in a ratio of 5g:2g:0.3g:4mL into a beaker and mix well to obtain an activation solution for later use;

[0030] Weigh: 10 g of pretreated carbon nanotubes and 70 mL of activation solution are added to a three-necked flask and stirred. The temperature of the three-necked flask is increased to 88°C at a heating rate of 0.3°C / min, and the temperature is kept for 2 hours. The temperature of the three-necked flask is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral. The filter cake is transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain activated nanotubes;

[0031] Weigh: 10 g of activated nanotubes, 37.5 mL of deionized water, 5.00 g of sodium vanadate and 5.16 g of titanium tetrachloride, add them into a three-necked flask and stir, add 12.5 mL of 6 mol / L hydrochloric acid dropwise into the three-necked flask, raise the temperature of the three-necked flask to 65°C, keep the temperature for 2 hours, lower the temperature of the three-necked flask to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake to a drying oven at 70°C, and dry it to constant weight to obtain modified nanotubes;

[0032] Add acetylene and nitrogen into the atmosphere furnace at a volume ratio of 1:19 to form a protective gas in the atmosphere furnace;

[0033] The modified nanotubes were added into an atmosphere furnace loaded with a protective gas atmosphere, the temperature of the atmosphere furnace was increased to 600°C at a heating rate of 5°C / min, and the temperature was kept for 4 hours. The atmosphere furnace was naturally cooled to room temperature to obtain composite carbon nanotubes.

[0034] S3. Preparation of conductive additives

[0035] Weigh: 4 g of cobalt acetate and 60 mL of ethylene glycol are added to a three-necked flask and stirred until the system is dissolved, 2.4 g of Tween 80 and 6 g of glucose are added to the three-necked flask, the temperature of the three-necked flask is raised to 120°C, and the mixture is stirred for 10 hours at this temperature, the temperature of the three-necked flask is lowered to room temperature, and the filter cake is filtered, and the filter cake is washed three times with anhydrous ethanol and then dried, and the filter cake is transferred to a drying oven at a temperature of 60°C and dried to constant weight to obtain caramelized glucose;

[0036] Weigh: 6g of caramelized glucose and 2g of sulfur powder, mix evenly and add into an argon-protected atmosphere furnace, raise the temperature of the atmosphere furnace to 650°C, keep warm for 4 hours, lower the temperature of the atmosphere furnace to room temperature, discharge the material, wash the calcined powder three times with methanol and then filter it, transfer the filter cake to a drying oven at a temperature of 55°C, dry it to constant weight, and obtain a conductive additive.

[0037] S4. Preparation of mixed slurry

[0038] Weigh: 14 g of composite nanotubes, 4 g of acetylene black, 2 g of conductive additive, 2 g of polyvinylidene fluoride and 8 mL of N-methylpyrrolidone, add into a beaker and mix to obtain a mixed slurry.

[0039] S5. Preparation of negative electrode materials

[0040] After the mixed slurry is evenly coated on the surface of the carbon fiber cloth, the carbon fiber cloth is transferred to a drying oven at a temperature of 60°C, vacuum dried to constant weight, and punched using a punching machine to obtain a negative electrode material with a diameter of 10 mm.

[0041] Example 2

[0042] The method for preparing the low temperature resistant and high rate sodium ion battery negative electrode material provided in this embodiment comprises the following steps:

[0043] S1. Preparation of pretreated carbon nanotubes

[0044] Weigh: 20 g of multi-walled carbon nanotubes and 2 g of nano-iron oxide powder are added to an atmosphere furnace at a temperature of 425°C, and air is introduced into the atmosphere furnace at a flow rate of 10 mL / min. The temperature is kept warm for 70 minutes, and the temperature of the atmosphere furnace is lowered to room temperature. Multi-walled carbon nanotubes and 5 mol / L hydrochloric acid are added to the flask in a dosage ratio of 1g:8mL and stirred. The temperature of the flask is increased to reflux of the system, and the temperature is kept warm for 4 hours. The temperature of the flask is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain pretreated carbon nanotubes.

[0045] S2. Preparation of composite nanotubes

[0046] Add 98wt% sulfuric acid, 65wt% nitric acid, potassium permanganate and hydrogen peroxide in a ratio of 5g:2g:0.3g:4mL into a beaker and mix well to obtain an activation solution for later use;

[0047] Weigh: 10 g of pretreated carbon nanotubes and 70 mL of activation solution are added to a three-necked flask and stirred. The temperature of the three-necked flask is increased to 90°C at a heating rate of 0.3°C / min, and the temperature is kept for 2.5 hours. The temperature of the three-necked flask is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral. The filter cake is transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain activated nanotubes;

[0048] Weigh: 10 g of activated nanotubes, 37.5 mL of deionized water, 5.00 g of sodium vanadate and 5.16 g of titanium tetrachloride, add them into a three-necked flask and stir, add 12.5 mL of 7 mol / L hydrochloric acid dropwise into the three-necked flask, raise the temperature of the three-necked flask to 70°C, keep the temperature for 2.5 hours, lower the temperature of the three-necked flask to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake to a drying oven at a temperature of 75°C, and dry it to constant weight to obtain modified nanotubes;

[0049] Add acetylene and nitrogen into the atmosphere furnace at a volume ratio of 1:19 to form a protective gas in the atmosphere furnace;

[0050] The modified nanotubes were added into an atmosphere furnace loaded with a protective gas atmosphere, the temperature of the atmosphere furnace was increased to 625°C at a heating rate of 5°C / min, and the temperature was kept for 5 hours. The atmosphere furnace was naturally cooled to room temperature to obtain composite carbon nanotubes.

[0051] S3. Preparation of conductive additives

[0052] Weigh: 4 g of cobalt acetate and 60 mL of ethylene glycol are added to a three-necked flask and stirred until the system is dissolved, 2.4 g of Tween 80 and 6 g of glucose are added to the three-necked flask, the temperature of the three-necked flask is raised to 125°C, and the mixture is stirred for 11 hours at this temperature, the temperature of the three-necked flask is lowered to room temperature, and the filter cake is filtered, and the filter cake is washed three times with anhydrous ethanol and then dried, and the filter cake is transferred to a drying oven at a temperature of 65°C and dried to constant weight to obtain caramelized glucose;

[0053] Weigh: 6g of caramelized glucose and 2g of sulfur powder, mix evenly and add into an argon-protected atmosphere furnace, raise the temperature of the atmosphere furnace to 670°C, keep warm for 5 hours, lower the temperature of the atmosphere furnace to room temperature, discharge the material, wash the calcined powder three times with methanol and then filter it, transfer the filter cake to a drying oven at a temperature of 60°C, dry it to constant weight, and obtain a conductive additive.

[0054] S4. Preparation of mixed slurry

[0055] Weigh: 14 g of composite nanotubes, 4 g of acetylene black, 2 g of conductive additive, 2 g of polyvinylidene fluoride and 8 mL of N-methylpyrrolidone, add into a beaker and mix to obtain a mixed slurry.

[0056] S5. Preparation of negative electrode materials

[0057] After the mixed slurry is evenly coated on the surface of the carbon fiber cloth, the carbon fiber cloth is transferred to a drying oven at a temperature of 65°C, vacuum dried to constant weight, and punched using a punching machine to obtain a negative electrode material with a diameter of 10 mm.

[0058] Example 3

[0059] The method for preparing the low temperature resistant and high rate sodium ion battery negative electrode material provided in this embodiment comprises the following steps:

[0060] S1. Preparation of pretreated carbon nanotubes

[0061] Weigh: 20 g of multi-walled carbon nanotubes and 2 g of nano-iron oxide powder are added to an atmosphere furnace at a temperature of 450°C, and air is introduced into the atmosphere furnace at a flow rate of 10 mL / min. The temperature is kept warm for 80 minutes, and the temperature of the atmosphere furnace is lowered to room temperature. Multi-walled carbon nanotubes and 5 mol / L hydrochloric acid are added to the flask in a dosage ratio of 1g:8mL and stirred. The temperature of the flask is increased to reflux of the system, and the temperature is kept warm for 5 hours. The temperature of the flask is lowered to room temperature, and the filter cake is washed with purified water until it is neutral and then dried. The filter cake is transferred to a drying oven at a temperature of 80°C and dried to constant weight to obtain pretreated carbon nanotubes.

[0062] S2. Preparation of composite nanotubes

[0063] Add 98wt% sulfuric acid, 65wt% nitric acid, potassium permanganate and hydrogen peroxide in a ratio of 5g:2g:0.3g:4mL into a beaker and mix well to obtain an activation solution for later use;

[0064] Weigh: 10 g of pretreated carbon nanotubes and 70 mL of activation solution are added to a three-necked flask and stirred. The temperature of the three-necked flask is increased to 92°C at a heating rate of 0.3°C / min, and the temperature is kept for 3 hours. The temperature of the three-necked flask is lowered to room temperature, filtered, and the filter cake is washed with purified water until it is neutral. The filter cake is transferred to a drying oven at a temperature of 80°C and dried to constant weight to obtain activated nanotubes;

[0065] Weigh: 10 g of activated nanotubes, 37.5 mL of deionized water, 5.00 g of sodium vanadate and 5.16 g of titanium tetrachloride, add them into a three-necked flask and stir, add 12.5 mL of 8 mol / L hydrochloric acid dropwise into the three-necked flask, raise the temperature of the three-necked flask to 75°C, keep the temperature for 3 hours, lower the temperature of the three-necked flask to room temperature, filter, wash the filter cake with purified water until it is neutral, transfer the filter cake to a drying oven at 80°C, and dry it to constant weight to obtain modified nanotubes;

[0066] Add acetylene and nitrogen into the atmosphere furnace at a volume ratio of 1:19 to form a protective gas in the atmosphere furnace;

[0067] The modified nanotubes were added into an atmosphere furnace loaded with a protective gas atmosphere, the temperature of the atmosphere furnace was increased to 650°C at a heating rate of 5°C / min, and the temperature was kept for 6 hours. The atmosphere furnace was naturally cooled to room temperature to obtain composite carbon nanotubes.

[0068] S3. Preparation of conductive additives

[0069] Weigh: 4 g of cobalt acetate and 60 mL of ethylene glycol are added to a three-necked flask and stirred until the system is dissolved, 2.4 g of Tween 80 and 6 g of glucose are added to the three-necked flask, the temperature of the three-necked flask is raised to 130°C, and the mixture is stirred for 12 hours at this temperature, the temperature of the three-necked flask is lowered to room temperature, and the filter cake is filtered, and the filter cake is washed three times with anhydrous ethanol and then dried, and the filter cake is transferred to a drying oven at a temperature of 70°C and dried to constant weight to obtain caramelized glucose;

[0070] Weigh: 6g of caramelized glucose and 2g of sulfur powder, mix evenly and add into an argon-protected atmosphere furnace, raise the atmosphere furnace temperature to 690°C, keep warm for 6h, lower the atmosphere furnace temperature to room temperature, discharge the material, wash the calcined powder three times with methanol and then filter, transfer the filter cake to a drying oven at a temperature of 65°C, dry to constant weight, and obtain a conductive additive.

[0071] S4. Preparation of mixed slurry

[0072] Weigh: 14 g of composite nanotubes, 4 g of acetylene black, 2 g of conductive additive, 2 g of polyvinylidene fluoride and 8 mL of N-methylpyrrolidone, add into a beaker and mix to obtain a mixed slurry.

[0073] S5. Preparation of negative electrode materials

[0074] After the mixed slurry is evenly coated on the surface of the carbon fiber cloth, the carbon fiber cloth is transferred to a drying oven at a temperature of 70°C, vacuum dried to constant weight, and punched using a punching machine to obtain a negative electrode material with a diameter of 10 mm.

[0075] Comparative Example 1

[0076] The difference between this comparative example and Example 1 is that step S2 is eliminated, and the composite nanotubes in step S4 are replaced by an equal amount of the pretreated carbon nanotubes obtained in step S1.

[0077] Comparative Example 2

[0078] The difference between this comparative example and Example 1 is that step S3 is omitted and no conductive additive is added in step S4.

[0079] Comparative Example 3

[0080] The difference between this comparative example and Example 1 is that steps S1-S2 are eliminated and no composite nanotubes are added in step S4.

[0081] Performance Test:

[0082] The negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-3 were used as working electrodes, sodium sheets were used as counter electrodes, glass fibers were used as separators, and the electrolyte was an EC-DEC solution of 1 mol / L NaClO4, wherein the volume ratio of EC:DEC was 1:1, to form sodium ion battery samples. According to the standard GB / T 24533-2019 "Graphite Negative Electrode Materials for Lithium Ion Batteries", the first discharge specific capacity, the first coulomb efficiency, and the discharge specific capacity after 100 cycles of the samples at room temperature and -20°C were measured, respectively, and the first discharge specific capacity, the first coulomb efficiency, and the discharge specific capacity of the samples after 100 cycles under 100C conditions were measured. The specific test results are shown in the following table:

[0083]

[0084]

[0085] Data Analysis:

[0086] Comparing and analyzing the data in the above table, the sodium ion battery sample prepared by the present invention has a specific capacity of 386 (mA·h)·g at room temperature and 1C for the first discharge. -1 At room temperature, the specific capacity of 1C100 discharges reaches 325 (mA·h)·g -1 After 100 cycles, the discharge capacity retention reached 84.38%, and the first coulombic efficiency reached 93.5%; at -20℃ and 1C, the first discharge capacity reached 303.7 (mA·h)·g -1 , at -20℃, 1C100 discharge capacity reaches 212.3 (mA·h)·g -1 After 100 cycles, the discharge capacity retention reached 69.91%, and the first coulombic efficiency reached 86.3%; at room temperature and 100C, the first discharge capacity reached 356.4 (mA·h)·g -1 At room temperature, 100C 100 times discharge capacity reaches 312.8 (mA·h)·g -1 After 100 cycles, the discharge capacity retention reaches 87.76%, and the first coulombic efficiency reaches 90.6%. All the test data are better than those of the comparative example, indicating that the negative electrode material prepared by the present invention has a good discharge capacity retention in a low temperature and high rate environment when applied in sodium ion batteries.

[0087] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0089] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material, characterized in that: The following steps are involved: S1, adding the pretreated carbon nanotubes and the activation solution into a three-necked flask and stirring, raising the temperature of the three-necked flask to 88-92°C at a heating rate of 0.3°C / min, keeping the temperature for 2-3h, and post-treating to obtain activated nanotubes, wherein the activation solution is composed of 98wt% sulfuric acid, 65wt% nitric acid, potassium permanganate and hydrogen peroxide in a dosage ratio of 5g:2g:0.3g:4mL; S2, adding activated nanotubes, deionized water, sodium vanadate and titanium tetrachloride into a three-necked flask and stirring, adding hydrochloric acid dropwise into the three-necked flask, raising the temperature of the three-necked flask to 65-75° C., keeping the temperature for reaction for 2-3 hours, and post-treating to obtain modified nanotubes; S3, adding the modified nanotubes into an atmosphere furnace loaded with a protective gas atmosphere, raising the temperature of the atmosphere furnace to 600-650°C at a heating rate of 5°C / min, and heat preservation for 4-6 hours, and naturally cooling the atmosphere furnace to room temperature to obtain composite carbon nanotubes, wherein the protective gas atmosphere is composed of acetylene and nitrogen in a volume ratio of 1:19; S4, adding the composite nanotubes, acetylene black, conductive additive, binder and N-methylpyrrolidone into a beaker for slurry mixing to obtain a mixed slurry, and evenly coating the mixed slurry on the surface of the carbon fiber cloth, and then post-treating to obtain a negative electrode material; The preparation method of pretreated carbon nanotubes is as follows: multi-walled carbon nanotubes and iron oxide are added into an atmosphere furnace at a temperature of 400-450°C, air is introduced into the atmosphere furnace at a flow rate of 10 mL / min, heat preservation treatment is performed for 60-80 minutes, and post-treatment is performed to obtain pretreated carbon nanotubes, wherein the post-treatment operation includes: after the reaction is completed, the temperature of the atmosphere furnace is reduced to room temperature, carbon nanotubes and 5 mol / L hydrochloric acid are added to a flask at a dosage ratio of 1g:8mL and stirred, the temperature of the flask is increased to reflux of the system, heat preservation treatment is performed for 3-5 hours, the temperature of the flask is reduced to room temperature, suction filtration is performed, the filter cake is washed with purified water until it is neutral and then dried, and the filter cake is transferred to a drying oven at a temperature of 70-80°C, and dried to constant weight to obtain pretreated carbon nanotubes; Conductive additives are processed by the following steps: A1. Add cobalt acetate and ethylene glycol into a three-necked flask and stir until the system is dissolved. Add Tween 80 and glucose into the three-necked flask. Raise the temperature of the three-necked flask to 120-130° C., keep warm and stir for 10-12 hours, and post-treat to obtain caramelized glucose. A2. Evenly mix caramelized glucose and sulfur powder and add them into an argon-protected atmosphere furnace. The temperature of the atmosphere furnace is raised to 650-690° C. and the mixture is kept warm for 4-6 hours. The conductive additive is obtained by post-processing.

2. The method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material according to claim 1, characterized in that: In step S1, the ratio of the pretreated carbon nanotubes to the activation solution is 1 g:7 mL, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is lowered to room temperature, filtered, the filter cake is washed with purified water until it is neutral, and the filter cake is transferred to a drying oven at a temperature of 70-80°C and dried to constant weight to obtain activated nanotubes.

3. The method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material according to claim 1, characterized in that: The weight ratio of the multi-walled carbon nanotubes to iron oxide is 10:

1.

4. The method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material according to claim 1, characterized in that: In step S2, the dosage ratio of sodium vanadate and titanium tetrachloride is 1 mol:1 mol, the dosage ratio of the activated nanotubes, deionized water, sodium vanadate and hydrochloric acid is 4 g:15 mL:2 g:5 mL, the concentration of the hydrochloric acid is 6-8 mol / L, and the post-treatment operation includes: after the reaction is completed, the temperature of the three-necked flask is lowered to room temperature, suction filtration is performed, the filter cake is washed with purified water until it is neutral, the filter cake is transferred to a drying oven at a temperature of 70-80° C., and dried to constant weight to obtain modified nanotubes.

5. The method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material according to claim 1, characterized in that: In step A1, the dosage ratio of cobalt acetate, ethylene glycol, Tween 80 and glucose is 1g:15mL:0.6g:1.5g, and the post-processing operation includes: after the reaction is completed, the temperature of the three-necked flask is reduced to room temperature, suction filtration is performed, the filter cake is washed three times with anhydrous ethanol and then dried, and the filter cake is transferred to a drying oven with a temperature of 60-70°C, and dried to constant weight to obtain caramelized glucose; in step A2, the weight ratio of caramelized glucose and sulfur powder is 3:1, and the post-processing operation includes: after the reaction is completed, the temperature of the atmosphere furnace is reduced to room temperature, the material is discharged, the calcined powder is washed three times with methanol and then suction filtered, and the filter cake is transferred to a drying oven with a temperature of 55-65°C, and dried to constant weight to obtain a conductive additive.

6. The method for preparing a low temperature resistant, high rate sodium ion battery negative electrode material according to claim 1, characterized in that: In step S4, the weight ratio of the composite nanotubes, acetylene black, conductive additive, binder and N-methylpyrrolidone is 7:2:1:1:4, the binder is polyvinylidene fluoride, and the post-processing operation includes: transferring the carbon fiber cloth coated with the mixed slurry to a drying oven at a temperature of 60-70°C, vacuum drying to constant weight, and using a punching machine to punch out to obtain a negative electrode material with a diameter of 10 mm.