Adsorbent for removing metal impurities in organic aminotin and preparation method thereof

By using a modified alumina adsorbent in organic amine tin, and combined with reduced pressure distillation, the decomposition and yield reduction problems in the prior art due to poor thermal stability are solved, and high-purity organic amine groups are achieved The preparation of tin improves the safety and yield of the product.

CN117718003BActive Publication Date: 2024-11-08HEFEI ADCHEM SEMI-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311712967.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2024-11-08
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

When the prior art improves the purity of organic amine-tin metal to 99.9999%, the decomposition and yield decrease due to poor thermal stability during distillation, and there are safety risks, making it difficult to effectively remove metal impurities.

Method used

Alumina is synthesized as the adsorbent for the carrier under nitrogen protection, and sulfonic acid groups and nitrogen-containing active groups are introduced through surface modification to adsorb metal impurities, and the metal purity of organic amine tin is improved by combining with reduced pressure distillation.

Benefits of technology

It effectively reduces the content of metal impurities in organic amine tin, improves metal purity to 99.9999%, avoids decomposition losses, and improves product yield and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004605308120000011
    Figure BDA0004605308120000011
Patent Text Reader

Abstract

The invention discloses an adsorbent for removing metal impurities in organic amino tin and a preparation method thereof, belongs to the technical field of organic amino tin synthesis, and comprises the following steps: under nitrogen protection, neutral aluminum oxide, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA and tetramethylethylenediamine are added to 4-methylpyridine, heated and stirred for 10-15h, cooled to room temperature, and then Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine are added, heated and stirred for 4-8h, cooled to room temperature, filtered, rinsed, drained, dried, and an adsorbent is obtained. The adsorbent prepared by the present invention uses aluminum oxide as a carrier, and by surface modification of the aluminum oxide carrier, while avoiding the carrier from reacting with the organic amino tin crude product, the effective adsorption of metal impurities is achieved, and after experimental verification, the organic amino tin crude product is subjected to adsorption treatment of the adsorbent, and the content of various metal impurities is significantly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic amine tin synthesis, and particularly relates to an adsorbent for removing metal impurities in organic amine tin and a preparation method thereof. Background Art

[0002] Organic aminotin, the general structural formula is Sn(NR1R2)4, as shown in the figure below:

[0003]

[0004] Wherein, R1 and R2 are the same or different straight chain or branched alkyl groups. Common organic amine tins on the market include tetra(dimethylamino)tin, tetra(methylethylamino)tin, tetra(diisopropylamino)tin, etc. Organic amine tins are used as precursors for CVD (Chemical Vapor Deposition) and ALD (Atomic Layer Deposition) deposition technologies in the semiconductor industry to prepare tin oxide films. In recent years, they have been widely concerned in the photovoltaic industry for their use in the research of perovskite solar cells with high-efficiency photoelectric conversion.

[0005] The most commonly used method for preparing organic amine tin is to directly react alkyl lithium with organic amine R1R2NH in the presence of a solvent to prepare organic amine lithium, then react with tin tetrachloride, further separate, and obtain an organic amine tin precursor of a certain purity through distillation and purification. For example, patent CN109988189A discloses a synthesis method of tetra(methylethylamino)tin, in which butyl lithium reacts with methylethylamine in an alkane solvent, and then tin tetrachloride is added to react, and after post-treatment, a certain purity of tetra(methylethylamino)tin crude product is obtained by vacuum distillation. Patent CN116947916A uses n-hexane as a solvent, butyl lithium reacts with dimethylamine, and then reacts with tin tetrachloride, and a crude product is obtained through post-treatment. After the crude product is distilled and purified, a tetra(dimethylamino)tin product with a metal purity of 99.999% is obtained. Patent CN116925130A takes into account the danger of using alkyl lithium reagents in process amplification, replaces the alkyl lithium reagent with a metal hydride, and replaces the solvent with a tetrahydrofuran solvent. Metal hydride and tin tetrachloride are added to the tetrahydrofuran solvent, and then dimethylamine is introduced. After reaction and post-treatment, a crude product is obtained. After distillation of the crude product, a product with a metal purity of 99.9999% can be obtained.

[0006] In the above patents, the purity of the crude organic amino tin product is generally between 99.9% and 99.99%. In order to obtain an organic amino tin product with a metal purity of >99.999%, the synthesized crude product is purified by distillation, but the thermal stability of the organic amino tin substance is poor. For example, tetra(dimethylamino)tin compounds will continue to decompose when heated at a temperature of >110°C for more than 20 hours in the presence of trace amounts of water and oxygen. Therefore, the distillation method has very high requirements for the sealing of the distillation equipment. On the one hand, in industrial amplification, due to the amplification of the product amount, the significant extension of the distillation time will cause the organic amino tin to continue to decompose, resulting in a reduction in yield, and the decomposition will continue to release heat, which poses certain safety hazards. At the same time, for compounds such as tetra(methylethylamino)tin and tetra(diisopropylamino)tin with higher boiling points, in order to obtain products with a metal purity of >99.9999%, the distillation yield will be greatly reduced due to thermal decomposition during the distillation purification process. Summary of the invention

[0007] In combination with the analysis of the above prior art, the present application aims to provide an adsorbent for simply and efficiently removing metal impurities from crude organic amino tin products. The synthesis process of the adsorbent is simple. The crude organic amino tin product is subjected to adsorption treatment using the adsorbent synthesized by the present invention. The metal purity of the crude organic amino tin product can be increased from 99.9% / 99.99% to ≥99.999%. After vacuum distillation, the purity can be further increased to ≥99.9999% of an electronic-grade organic amino tin product.

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] The preparation method of an adsorbent for removing metal impurities in organic amino tin comprises the following steps:

[0010] S1. Under nitrogen protection, add neutral alumina, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA and tetramethylethylenediamine to 4-methylpyridine, start stirring and heating, control the temperature at 130°C-140°C, and stir the reaction for 10-15h;

[0011] S2, the reaction temperature is cooled to room temperature, and Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine are added, stirring and heating are started, the temperature is controlled at 90-100°C, and the reaction is stirred for 4-8h;

[0012] S3. The reaction mixture is cooled to room temperature, filtered, and the filtered solid is rinsed with n-hexane three times, dried, and then dried at 110-130° C. under negative pressure to obtain an adsorbent.

[0013] Furthermore, the usage ratio of 4-methylpyridine, neutral alumina, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA, tetramethylethylenediamine, Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine is 1000mL:490-520g:9-12g:18-25g:18-22g:45-55g:4.5-5.5g:4-6g.

[0014] Furthermore, the particle size of the neutral alumina is 100-200 mesh.

[0015] Furthermore, the negative pressure is -0.095Mpa-(-0.099Mpa).

[0016] Beneficial effects of the present invention:

[0017] The present invention prepares an adsorbent for removing metal impurities in organic amino tin. The adsorbent uses aluminum oxide as a carrier. The present invention performs surface modification on the aluminum oxide carrier. On the one hand, by modifying the surface active points, the reaction between the carrier and the organic amino tin crude product is avoided, resulting in the decomposition and destruction of the organic amino tin crude product itself. On the other hand, the present invention achieves effective adsorption of metal impurities by introducing sulfonic acid groups that can adsorb metal impurities and different nitrogen-containing active groups that have adsorption effects on different metal impurities on the surface of the aluminum oxide carrier. Experimental verification shows that the contents of various metal impurities are significantly reduced after the organic amino tin crude product is adsorbed by the adsorbent. The adsorbent prepared by the present invention is suitable for various organic amino tin compounds. After the organic amino tin crude product is treated, there is basically no loss to obtain an organic amino tin compound with a metal purity of more than 99.9999%. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1

[0020] Preparation of an adsorbent for removing metal impurities in organic amino tin comprises the following steps:

[0021] S1. Under nitrogen protection, add 1000 mL of 4-methylpyridine, 490 g of 100-200 mesh neutral alumina, 9 g of sodium dodecylbenzenesulfonate, 18 g of N-methylpyrrolidone, 18 g of disodium EDTA and 45 g of tetramethylethylenediamine to a 2L reaction bottle, start stirring and heating, control the reaction temperature to 130°C, and stir the reaction for 10 hours;

[0022] S2, the reaction temperature was cooled to room temperature, and under nitrogen protection, 4.5 g of Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 4 g of 2-(2-thienyl)pyridine were added to the reaction bottle, stirring and heating were started, the heating temperature was controlled at 90°C, and the stirring reaction was continued for 4 h;

[0023] S3, the reaction mixture was cooled to room temperature, filtered, and the filtered solid was rinsed with n-hexane 3 times, each time with 1000 mL of n-hexane, and finally the filtered solid was drained;

[0024] S4. The filtered solid is transferred into a drying oven, the oven temperature is set to 110°C, and the filtered solid is dried under negative pressure (-0.095Mpa to -0.099Mpa) for 12 hours;

[0025] S5. The dried solid product is sealed and stored in a glove box.

[0026] Example 2

[0027] Preparation of an adsorbent for removing metal impurities in organic amino tin comprises the following steps:

[0028] S1. Under nitrogen protection, add 1000 mL of 4-methylpyridine, 500 g of 100-200 mesh neutral alumina, 10 g of sodium dodecylbenzenesulfonate, 20 g of N-methylpyrrolidone, 20 g of disodium EDTA and 50 g of tetramethylethylenediamine to a 2L reaction bottle, start stirring and heating, control the reaction temperature at 130°C-140°C, and stir the reaction for 12 hours;

[0029] S2, the reaction temperature was cooled to room temperature, and under nitrogen protection, 5 g of Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 5 g of 2-(2-thienyl)pyridine were added to the reaction bottle, stirring and heating were started, the heating temperature was controlled at 90-100°C, and the stirring reaction was continued for 5 h;

[0030] S3, the reaction mixture was cooled to room temperature, filtered, and the filtered solid was rinsed with n-hexane 3 times, each time with 1000 mL of n-hexane, and finally the filtered solid was drained;

[0031] S4. The filtered solid is transferred into a drying oven, the oven temperature is set to 120°C, and the filtered solid is dried under negative pressure (-0.095Mpa to -0.099Mpa) for 12 hours;

[0032] S5. The dried solid product is sealed and stored in a glove box.

[0033] Example 3

[0034] Preparation of an adsorbent for removing metal impurities in organic amino tin comprises the following steps:

[0035] S1. Under nitrogen protection, add 1000 mL of 4-methylpyridine, 520 g of 100-200 mesh neutral alumina, 12 g of sodium dodecylbenzenesulfonate, 25 g of N-methylpyrrolidone, 22 g of disodium EDTA and 55 g of tetramethylethylenediamine to a 2L reaction bottle, start stirring and heating, control the reaction temperature to 140 ° C, and stir the reaction for 15 hours;

[0036] S2, the reaction temperature was cooled to room temperature, and under nitrogen protection, 5.5 g of Boc-N-(2-chlorobenzyloxycarbonyl)-D-lysine and 6 g of 2-(2-thienyl)pyridine were added to the reaction bottle, stirring and heating were started, the heating temperature was controlled at 100°C, and the stirring reaction was continued for 8 h;

[0037] S3, the reaction mixture was cooled to room temperature, filtered, and the filtered solid was rinsed with n-hexane 3 times, each time with 1000 mL of n-hexane, and finally the filtered solid was drained;

[0038] S4. The filtered solid is transferred into a drying oven, the oven temperature is set to 130°C, and the filtered solid is dried under negative pressure (-0.095Mpa to -0.099Mpa) for 24 hours;

[0039] S5. The dried solid product is sealed and stored in a glove box.

[0040] Example 4

[0041] The adsorbent is applied to the adsorption of metal impurities in the synthesis of organic aminotin, comprising the following steps:

[0042] The crude organic aminotin product is 500 g of tetrakis(dimethylamino)tin crude product, and the metal purity is 99.9% (the impurities are mainly metallic lithium, and the metallic lithium content is 80-100 ppm). Under nitrogen protection, 20 g of the adsorbent prepared in Example 2 is added to a clean chromatography column, and 500 g of the tetrakis(dimethylamino)tin crude product is slowly passed through the adsorbent by a column chromatography separation method, and the outflow rate is controlled to be about 100 mL / h. The column liquid is collected at the lower end of the chromatography column with a clean glass container, and finally Then, the tetra(dimethylamino)tin product in the adsorbent was pressed into a collection container with a slight nitrogen gas, and the tetra(dimethylamino)tin filtrate after adsorption was sampled and tested by ICPMS, and the metal purity was >99.999% (the metallic lithium content was 0.30ppm). The tetra(dimethylamino)tin filtrate was subjected to rapid reduced pressure distillation to obtain qualified tetra(dimethylamino)tin products, and the metal purity was >99.9999% (the impure metallic lithium content was 0.03ppm) after sampling and ICPMS testing.

[0043] Example 5

[0044] The adsorbent is applied to the adsorption of metal impurities in the synthesis of organic aminotin, comprising the following steps:

[0045] The crude organic aminotin product is 3000g of tetra(dimethylamino)tin crude product, with a metal purity of 99.99% (the impurity is mainly metallic lithium, with a metallic lithium content of 15ppm). Under nitrogen protection, 40g of adsorbent is added to a clean chromatography column, and 3000g of tetra(dimethylamino)tin crude product is slowly passed through the adsorbent by column chromatography separation method, and the outflow rate is controlled to be about 200mL / h. The column liquid is collected in a clean glass container at the lower end of the chromatography column, and finally the column liquid is separated by a slight nitrogen The tetra(dimethylamino)tin product in the adsorbent is pressed into a collecting container by gas. The filtrate of the adsorbed tetra(dimethylamino)tin is sampled and tested by ICPMS. The metal purity is>99.999% (the metallic lithium content is 0.26ppm). The filtrate of the tetra(dimethylamino)tin is subjected to rapid reduced pressure distillation to obtain qualified tetra(dimethylamino)tin products. The metal purity is>99.9999% (the impure metallic lithium content is 0.04ppm) by ICPMS.

[0046] Example 6

[0047] The adsorbent is applied to the adsorption of metal impurities in the synthesis of organic aminotin, comprising the following steps:

[0048] The crude organic amino tin product is 800 g of crude tetra(methylethylamino)tin, with a metal purity of 99.9% (impurities are mainly metallic lithium and sodium, with a metallic lithium content of 150 ppm and a sodium content of 20 ppm). Under nitrogen protection, 20 g of adsorbent is added to a clean chromatography column, and 800 g of crude tetra(methylethylamino)tin is slowly passed through the adsorbent by a column chromatography separation method, with an outflow rate of about 100 mL / h. The column liquid is collected in a clean glass container at the lower end of the chromatography column, and the adsorbent is finally separated by a slight nitrogen gas. The medium tetra(methylethylamino)tin product was pressed into a collection container, and the filtrate of the adsorbed tetra(methylethylamino)tin was sampled and tested by ICPMS, and the metal purity was >99.999% (the metal lithium content was 0.3ppm and the sodium content was 0.1ppm). The filtrate of the tetra(methylethylamino)tin was subjected to rapid reduced pressure distillation to obtain qualified tetra(methylethylamino)tin products, and the metal purity was >99.9999% (the impurity metal lithium content was 0.02ppm and the sodium content was 0.01ppm).

[0049] Example 7

[0050] The adsorbent is applied to the adsorption of metal impurities in the synthesis of organic aminotin, comprising the following steps:

[0051] The crude organic amino tin product is 2000g of tetra(diethylamino)tin crude product, with a metal purity of 99.9% (impurities are mainly metallic lithium, sodium and potassium, with a metallic lithium content of 50ppm, a sodium content of 50ppm and a potassium content of 40ppm). Under nitrogen protection, 40g of adsorbent is added to a clean chromatography column, and 2000g of tetra(diethylamino)tin crude product is slowly passed through the adsorbent by a column chromatography separation method, and the outflow rate is controlled to be about 200mL / h. The column liquid is collected in a clean glass container at the lower end of the chromatography column, and finally the tetra(diethylamino)tin in the adsorbent is separated by a slight nitrogen gas. The tetra(diethylamino)tin product was pressed into a collection container, and the tetra(diethylamino)tin filtrate after adsorption was sampled and tested by ICPMS, and the metal purity was >99.999% (the metal lithium content was 0.4ppm, the sodium content was 0.1ppm, and the potassium content was 0.1ppm). The tetra(diethylamino)tin filtrate was subjected to rapid reduced pressure distillation to obtain a qualified tetra(diethylamino)tin product, and the sampled ICPMS test showed that the metal purity was >99.9999% (the impurity metal lithium content was 0.01ppm, the sodium content was 0.02ppm, and the potassium content was 0.01ppm).

[0052] Example 8

[0053] The adsorbent is applied to the adsorption of metal impurities in the synthesis of organic aminotin, comprising the following steps:

[0054] The crude organic aminotin product is 300g of tetrakis(diisopropylamino)tin crude product, and the metal purity is 99.9% (the impurities are mainly metallic lithium, and the metallic lithium content is 200ppm). Under nitrogen protection, 15g of adsorbent is added to a clean chromatography column, and 300g of tetrakis(methylethylamino)tin crude product is slowly passed through the adsorbent by column chromatography separation method, and the outflow rate is controlled to be about 50mL / h. The column liquid is collected in a clean glass container at the lower end of the chromatography column, and finally the tetrakis(diisopropylamino)tin in the adsorbent is separated by a slight nitrogen gas. ) The tin product was pressed into a collection container, and the filtrate of tetrakis(diisopropylamino)tin after adsorption was sampled and tested by ICPMS, and the metal purity was >99.999% (the content of metallic lithium was 0.4ppm, and the content of sodium was 0.09ppm). The filtrate of tetrakis(diisopropylamino)tin was subjected to rapid reduced pressure distillation to obtain qualified tetrakis(diisopropylamino)tin products, and the sampled ICPMS test showed that the metal purity was >99.9999% (the content of impure metallic lithium was 0.02ppm, and the content of metallic sodium was 0.01ppm).

[0055] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, and the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing an adsorbent for removing metal impurities from organic aminotin. It is characterized in that The following steps are involved: S1. Under nitrogen protection, add 4-methylpyridine, neutral alumina, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA and tetramethylethylenediamine to the reaction bottle, start stirring and heating, control the temperature at 130°C-140°C, and stir the reaction for 10-15h; S2, the reaction temperature is cooled to room temperature, and under nitrogen protection, Boc-N'-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine are added to the reaction bottle, stirring and heating are started, the temperature is controlled at 90-100°C, and the reaction is stirred for 4-8h; S3, the reaction mixture is cooled to room temperature, filtered, the filtered solid is rinsed with n-hexane three times, dried, and then dried at 110-130° C. under negative pressure to obtain an adsorbent; The usage ratio of the 4-methylpyridine, neutral alumina, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA, tetramethylethylenediamine, Boc-N´-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine is 1000mL: 490-520g: 9-12g: 18-25g: 18-22g: 45-55g: 4.5-5.5g: 4-6g.

2. The method for preparing an adsorbent for removing metal impurities in organic amino tin according to claim 1, It is characterized in that The dosage ratio of the 4-methylpyridine, neutral alumina, sodium dodecylbenzenesulfonate, N-methylpyrrolidone, disodium EDTA, tetramethylethylenediamine, Boc-N´-(2-chlorobenzyloxycarbonyl)-D-lysine and 2-(2-thienyl)pyridine is 1000mL:500g:10g:20g:20g:50g:5g:5g.

3. The method for preparing an adsorbent for removing metal impurities in organic amino tin according to claim 1, It is characterized in that The particle size of the neutral alumina is 100-200 meshes.

4. The method for preparing an adsorbent for removing metal impurities in organic amino tin according to claim 1, It is characterized in that The negative pressure is -0.095MPa-(-0.099MPa).

5. Adsorbent used to remove metal impurities in organic amino tin, It is characterized in that Prepared by the preparation method described in any one of claims 1 to 4.