Alloy material for preparing dumbbell pin and dumbbell pin thereof
By using specific alloy materials and corrosion-resistant layers, the problems of insufficient tensile strength of dumbbell pins and prone to rust on the surface are solved, the yield and strength ratio and corrosion resistance are improved, and the normal operation of the scraper chain and the safety of the equipment are ensured.
Patent Information
- Application Number
- CN202311645552.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-12-04
AI Technical Summary
The existing dumbbell pin materials have insufficient tensile strength and are prone to deformation, resulting in excessive gap between the chutes, affecting the normal operation of the scraper chain, and the surface is prone to rust and affecting the service life and experience.
Using an alloy material, including C, Si, Mn, Cr, Ni, Mo, V, B, Al, P, S, etc., through electric furnace smelting, diffusion heat treatment, forging, die forging, normalization, annealing and adjustment Made of heat treatment, the surface is coated with a corrosion-resistant layer to improve corrosion resistance.
It improves the yield and corrosion resistance of dumbbell pins, reduces deformation, avoids large damage to the chute gap, and enhances the safety and user experience of the equipment.
Smart Images

Figure CN117721396B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dumbbell pin preparation, and particularly relates to an alloy material used for preparing a dumbbell pin and a dumbbell pin thereof. Background Art
[0002] The scraper conveyor is composed of three parts: the head, the middle part and the tail part. The head part is composed of the head frame, the motor, the hydraulic coupling, the reducer and the sprocket; the middle part is composed of the transition trough, the middle trough, the chain and the scraper; the tail part is the device for the scraper chain to return. When the scraper conveyor is working, the head transmission part drives the sprocket on the head shaft to rotate, so that the scraper chain circulates and drives the material to move along the chute. The open chute serves as a bearing for coal, gangue or materials. The dumbbell pin, also known as the connecting pin, is an important component for connecting the chute on the scraper. A fully mechanized scraper is usually equipped with about 300 dumbbell pins. It has two functions: first, it prevents the chute from moving longitudinally and horizontally during the operation of the machine to ensure the normal operation of the scraper chain on the machine; second, it can break immediately when the scraper chain works abnormally or is overloaded, which plays a role in protecting the chute. The existing dumbbell pin material is generally 40CrNiMo. The dumbbell pin produced with this material has a tensile strength that can meet the use requirements, but the yield strength ratio is low, and a large elongation will occur before breaking, resulting in excessive chute gaps, causing chute deformation or the scraper chain to fail to operate normally. In addition, the surface of the existing dumbbell pin is made of cast iron material and is easily rusted, which not only affects the service life of the dumbbell pin, but also the generated rust easily affects the user experience. Summary of the invention
[0003] In view of the above problems, the present invention provides an alloy material for preparing a dumbbell pin and a dumbbell pin thereof, which can not only meet the strength requirements but also have a large yield strength ratio, thereby solving the problem of large deformation of the existing dumbbell pin before fracture. A corrosion-resistant layer is coated on the surface of the obtained dumbbell pin, thereby solving the problem of easy rust on the surface of the existing dumbbell pin.
[0004] The first object of the present invention is to provide an alloy material for preparing a dumbbell pin, which comprises the following chemical components by weight: C is 0.35-0.55%; Si is 0.70-1.50%; Mn is 0.70-1.50%; Cr is 0.10-2.00%; Ni is 0.10-0.50%; Mo is 0.05-0.50%; V is 0.01-0.50%; B is 0.01-0.50%; Al is 0.020-0.050%; P is ≤0.025%; S is ≤0.015; and the rest is Fe.
[0005] Furthermore, the alloy material is made by the following steps: electric furnace smelting or converter smelting, refining and vacuum treatment; electroslag remelting; diffusion heat treatment; forging blanking; die forging; normalizing treatment; annealing treatment and tempering heat treatment.
[0006] Furthermore, the process parameters of the diffusion heat treatment are: heating temperature of 1180℃~1300℃, keeping temperature for 5~15 hours; the process parameters of forging blanking are: cooling the steel ingot after diffusion heat treatment to a temperature range of 1100℃~1250℃ for forging blanking, and the final forging temperature is ≥900℃; the process parameters of die forging forming are: forming temperature of 950℃~1050℃.
[0007] Furthermore, the process parameters of the normalizing treatment are: heating temperature of 900°C to 920°C, holding time of 5 to 10 hours, and after cooling, the steel is placed in an annealing furnace and kept at 300°C for 5 to 10 hours; the process parameters of the annealing treatment are: annealing temperature of 660°C to 680°C, and holding time of 10 to 30 hours; the process parameters of the tempering heat treatment are: quenching temperature of 880°C to 900°C, holding time of 5 to 10 hours, and cooling to below 150°C with quenching liquid or oil; followed by tempering treatment at 400 to 600°C, and holding time of 10 to 20 hours.
[0008] A second object of the present invention is to provide a dumbbell pin comprising the above alloy material.
[0009] In some specific embodiments of the present invention, the dumbbell pin further includes a corrosion-resistant layer coated on the surface of the alloy material.
[0010] Furthermore, the corrosion-resistant layer comprises the following raw materials in parts by weight: 40-50 parts of silica sol, 20-35 parts of methyltrimethoxysiloxane, 10-30 parts of deionized water, 5-15 parts of ethanol, 5-9 parts of corrosion-resistant agent, and 0.5-1.5 parts of formic acid.
[0011] Furthermore, the corrosion inhibitor is prepared by a hyperbranching reaction of corrosion-resistant triol and adipic acid, and the number average molecular weight of the corrosion inhibitor is 1500-2000.
[0012] Furthermore, the molar ratio of the corrosive triol to adipic acid is 2-4:3-4.
[0013] Furthermore, the corrosion-resistant triol is prepared by heating 6-amino-3-pyridylmethanol and 2,2-dihydroxymethylpropionic acid in an organic solvent DMF to 90-100° C. and reacting for 3-12 hours under the action of a condensation reagent.
[0014] Beneficial effects of the present invention:
[0015] The alloy material and dumbbell pin for preparing the dumbbell pin provided by the present invention have excellent ratio of alloy elements, pure steel, uniform structure, stable performance and high yield strength ratio; the deformation is small when the strength required by the equipment is not exceeded, which can not only play the role of connection and fixing, but also avoid the damage of the chute due to large gap; when the scraper chain works abnormally or is overloaded, it will break immediately under very small deformation, which can effectively avoid major equipment safety accidents;
[0016] In order to improve the corrosion resistance and usage experience of the dumbbell pin made of the alloy material, the present invention coats a corrosion-resistant layer on the surface of the formed alloy material. The corrosion-resistant layer not only greatly improves the corrosion resistance of the dumbbell pin, but also improves the adhesion between the corrosion layer and the alloy material due to the coordination effect between the pyridine nitrogen in the corrosion-resistant triol and the metal of the alloy material.
[0017] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0019] Figure 1 A broken view of a dumbbell pin without a corrosion-resistant layer according to Example 1 of the present invention is shown;
[0020] Figure 2 A broken picture of a dumbbell pin without a corrosion-resistant layer according to Comparative Example 1 of the present invention is shown. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] An alloy material for preparing a dumbbell pin according to an embodiment of the present invention includes the following chemical components by weight: C is 0.35-0.55%; Si is 0.70-1.50%; Mn is 0.70-1.50%; Cr is 0.10-2.00%; Ni is 0.10-0.50%; Mo is 0.05-0.50%; V is 0.01-0.50%; B is 0.01-0.50%; Al is 0.020-0.050%; P is ≤0.025%; S is ≤0.015; and the rest is Fe.
[0023] In an embodiment of the present invention, the alloy material is made by the following steps: electric furnace smelting or converter smelting, refining and vacuum treatment; electroslag remelting; diffusion heat treatment; forging blanking; die forging; normalizing treatment; annealing treatment and tempering heat treatment.
[0024] In the embodiment of the present invention, smelting: electric furnace smelting or converter smelting, refining (LF) and vacuum treatment (VD) are carried out according to the chemical composition and mass percentage of the alloy material, and then electroslag remelting is carried out.
[0025] Among them, electric furnace smelting: the ingredients are prepared according to the chemical composition and mass percentage of the alloy material, high power is sent during the melting period, the temperature is quickly raised and oxidized, and the steel tapping temperature is 1600°C-1620°C;
[0026] Refining (LF): Add 0.8-1 kg / T of Al and SiC powder into the ladle, heat to 1550℃-1570℃, refining time ≥15 minutes, take samples to test chemical composition;
[0027] Vacuum treatment (VD): After the chemical composition is qualified, the molten steel is heated to 1600℃-1620℃ and enters the vacuum station for vacuuming. The vacuum degree is ≤150Torr and maintained for more than 15 minutes. The argon flow rate during vacuuming is 50-100NL / min. After breaking the vacuum, 0.3Kg / T of Al is added. When the molten steel temperature is 1550℃-1570℃, steel is cast;
[0028] Electroslag remelting: Φ250X1600mm graphite electrode is used to make slag, and the arc is started by conductive slag. The slag amount is 110 kg, including 66 kg of fluorite, 38 kg of alumina powder, and 6 kg of magnesia. The no-load voltage is 61V.
[0029] Slag making time: 0A-3500A slag making 20min, 6000A-7000A refining 30min;
[0030] Remelting voltage: 73V; current: 8000A after the first set of electrodes enter, increased to 13000A in 20 minutes, 12000A after the second set, and 11500 for the last half set; mold cooling time is 50 minutes, and the steel ingot is slowly cooled in the pit for 72 hours.
[0031] In an embodiment of the present invention, the process parameters of the diffusion heat treatment are: a heating temperature of 1180°C to 1300°C, and a heat preservation time of 5 to 15 hours. In a specific example, the specific temperature value in the diffusion heat treatment is any one of 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, 1250°C, 1260°C, 1270°C, 1280°C, 1290°C, and 1300°C, and the heat preservation time in the diffusion heat treatment is any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, and 15 hours.
[0032] In an embodiment of the present invention, the process parameters of the forging blanking are: the steel ingot that has undergone diffusion heat treatment is cooled to a temperature range of 1100°C to 1250°C for forging blanking, and the final forging temperature is ≥900°C. In a specific example, the specific temperature value of the steel ingot cooling during the forging blanking is any one of 1110°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C, and 1250°C.
[0033] In an embodiment of the present invention, the process parameters of the die forging are: after forging, a friction press is used for forging, and the forming temperature is 950°C to 1050°C. The specific value of the forming temperature in the die forging is any one of 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, and 1050°C.
[0034] In an embodiment of the present invention, the process parameters of the normalizing treatment are: a heating temperature of 900°C to 920°C, a holding time of 5 to 10 hours, and after cooling, the annealing furnace is placed at 300°C for 5 to 10 hours. The specific temperature value in the normalizing treatment is any one of 900°C, 905°C, 910°C, 915°C, and 920°C. The holding time in the normalizing treatment is any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours. The value of the holding time at 300°C is any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours.
[0035] In an embodiment of the present invention, the process parameters of the annealing treatment are: an annealing temperature of 660-680°C, a holding time of 10-30 hours, the specific value of the annealing temperature in the annealing treatment is any one of 600°C, 610°C, 920°C, 630°C, 640°C, 650°C, 660°C, 670°C, and 680°C, and the holding time is any one of 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours, and 30 hours.
[0036] In an embodiment of the present invention, the process parameters of the quenching and tempering heat treatment are: quenching temperature is 880°C to 900°C, holding time is 5 to 10 hours, and quenching liquid or oil is used to cool to below 150°C; then tempering treatment is performed at 400 to 600°C, and the holding time is 10 to 20 hours. The specific value of the quenching temperature in the quenching and tempering heat treatment is any one of 880°C, 885°C, 890°C, 895°C, and 900°C, and the specific value of the quenching holding time is any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours. The tempering treatment is performed at 400 to 600°C and the holding time is 10 to 20 hours. The specific value of the annealing temperature is any one of 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C and 600°C, and the specific value of the annealing holding time is any one of 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours and 20 hours.
[0037] In an embodiment of the present invention, a dumbbell pin is further provided, comprising the above alloy material.
[0038] In other embodiments of the present invention, the dumbbell pin further comprises a corrosion-resistant layer coated on the surface of the alloy material;
[0039] The corrosion-resistant layer comprises the following raw materials in parts by weight: 40-50 parts of silica sol, 20-35 parts of methyltrimethoxysiloxane, 10-30 parts of deionized water, 5-15 parts of ethanol, 5-9 parts of corrosion-resistant agent, and 0.5-1.5 parts of formic acid.
[0040] In the embodiment of the present invention, the silica sol is an alkaline silica sol with a pH value of 9-10 and a SiO2 mass fraction of 50%.
[0041] In an embodiment of the present invention, the corrosion inhibitor is formed by a hyperbranching reaction of corrosion-resistant triol and adipic acid, and the number average molecular weight of the corrosion inhibitor is 1500-2000.
[0042] In an embodiment of the present invention, the molar ratio of the corrosion-resistant triol to adipic acid in the hyperbranched reaction is 2-4:3-4, the hyperbranched reaction is a solvent reaction, and the solvent used is an organic solvent, the purpose of which is to promote the mixing of the corrosion-resistant triol and adipic acid, and the organic solvent is a reaction solvent for alcohols and organic acids well known in the technical field, such as toluene, benzene, cyclohexane, etc. The hyperbranched reaction requires the presence of a catalyst, and the catalyst is a catalyst for the reaction of alcohols and organic acids well known to personnel in the technical field, such as p-toluenesulfonic acid, concentrated sulfuric acid (mass fraction 98%), etc. The reaction temperature of the hyperbranched reaction is 85-100°C, and the reaction time is 4-24h.
[0043] In an embodiment of the present invention, the corrosion-resistant triol is prepared by heating 6-amino-3-pyridylmethanol and 2,2-dihydroxymethylpropionic acid in an organic solvent DMF under the action of a condensation reagent (such as DCC, EDC, DIC, HATU, etc.) to 90-100° C. and reacting for 3-12 hours, and the molar ratio of the 6-amino-3-pyridylmethanol and 2,2-dihydroxymethylpropionic acid is 1:1.
[0044] In an embodiment of the present invention, the preparation process of the corrosion-resistant layer comprises the following steps:
[0045] After mixing the weight parts of raw materials for the corrosion-resistant layer, stir at room temperature for 6-24 hours, then filter, spray on the surface of the pretreated forming alloy material, dry and solidify to obtain, wherein the drying temperature is 60-70°C, the drying time is 10-30min, the curing temperature is 100-150°C, and the curing time is 10-15min. The pretreated forming alloy material is obtained by grinding, cleaning and drying the forming alloy material.
[0046] Examples 1-5 and Comparative Example 1: Preparation of dumbbell pins without corrosion-resistant coating
[0047] According to Table 1, the chemical components of Examples 1 to 5 and Comparative Example 1 were taken and then prepared according to the following process parameters:
[0048] Smelting: carrying out batching electric furnace smelting or converter smelting, refining (LF) and vacuum treatment (VD) according to the chemical composition and mass percentage of the alloy material, and then carrying out electroslag remelting;
[0049] Among them, electric furnace smelting: the ingredients are prepared according to the chemical composition and mass percentage of the alloy material, high power is sent during the melting period, the temperature is quickly raised and oxidized, and the steel tapping temperature is 1600°C-1620°C;
[0050] Refining (LF): Add 0.8-1 kg / T of Al and SiC powder into the ladle, heat to 1550℃-1570℃, refining time ≥15 minutes, take samples to test chemical composition;
[0051] Vacuum treatment (VD): After the chemical composition is qualified, the molten steel is heated to 1600℃-1620℃ and enters the vacuum station for vacuuming. The vacuum degree is ≤150Torr and maintained for more than 15 minutes. The argon flow rate during vacuuming is 50-100NL / min. After breaking the vacuum, 0.3Kg / T of Al is added. When the molten steel temperature is 1550℃-1570℃, steel is cast;
[0052] Electroslag remelting: Φ250X1600mm graphite electrode is used to make slag, and the arc is started by conductive slag. The slag amount is 110 kg, including 66 kg of fluorite, 38 kg of alumina powder, and 6 kg of magnesia. The no-load voltage is 61V.
[0053] Slag making time: 0A-3500A slag making 20min, 6000A-7000A refining 30min;
[0054] Remelting voltage: 73V; current: 8000A after the first set of electrodes enter, increased to 13000A in 20 minutes, 12000A after the second set, and 11500 for the last half set; mold cooling time is 50 minutes, and the steel ingot is slowly cooled in the pit for 72 hours.
[0055] The process parameters of the diffusion heat treatment are: heating temperature is 1180°C, and heat preservation is 12 hours;
[0056] Forging and blanking: The steel ingot after diffusion heat treatment is cooled to 1150℃, and then forged and blanked, and the final forging temperature is ≥900℃;
[0057] Die forging: After forging, the blank is forged using a friction press, with a forming temperature of 1000°C;
[0058] Normalizing treatment: heating temperature is 900℃, holding time is 8 hours, after cooling, put into annealing furnace and hold at 300℃ for 6 hours;
[0059] Annealing treatment: annealing temperature is 670℃, holding time is 24 hours;
[0060] Quenching and tempering heat treatment: quenching temperature is 900℃, holding time is 7 hours, and quenching liquid or oil is used to cool to below 150℃; then tempering treatment is carried out at 500℃, holding time is 12 hours.
[0061] Table 1
[0062]
[0063] Examples 1-5 and Comparative Example 1 were subjected to breaking tests, and the experimental data are shown in Table 2. Figure 1 The following is a diagram of the broken dumbbell pin of Example 1 without the corrosion-resistant layer. Figure 2 A broken picture of a dumbbell pin without a corrosion-resistant layer is shown in Comparative Example 1.
[0064] Table 2
[0065]
[0066]
[0067] It can be seen from the experimental data in Table 2 that, compared with the traditional dumbbell pin material of Comparative Example 1, the deformation of Examples 1-5 of the present invention is smaller under the same breaking strength. In addition, under low load conditions, Examples 1-5 have almost no elongation, which can better avoid damage to the chute due to large gaps. When the scraper chain works abnormally or is overloaded, it will break immediately under very small deformation, which plays a better role in protecting the equipment.
[0068] Examples 6-10 and Comparative Example 2: Preparation of Dumbbell Pins with Surface-Coated Corrosion-Resistant Layers
[0069] The corrosion-resistant layer coated on the surface of the formed alloy material obtained in Example 1-5 (i.e., the dumbbell pin without the corrosion-resistant layer) is coated according to the following method:
[0070] The weight parts of raw materials for the corrosion-resistant layer are stirred and mixed, stirred at room temperature for 12 hours, then filtered, sprayed on the surface of the polished, cleaned and dried formed alloy material, dried and cured to obtain the product, wherein the drying temperature is 60°C, the drying time is 30 minutes, the curing temperature is 100°C, and the curing time is 15 minutes;
[0071] The corrosion-resistant layer comprises the following raw materials in parts by weight: 50 parts of silica sol, 30 parts of methyltrimethoxysiloxane, 20 parts of deionized water, 7 parts of ethanol, 6 parts of corrosion-resistant agent, and 1 part of formic acid;
[0072] The corrosion resistant agent is prepared according to the following steps:
[0073] 1. Preparation of corrosion-resistant triol: 6-amino-3-pyridylmethanol and 2,2-dihydroxymethylpropionic acid are added to an organic solvent DMF at a molar ratio of 1:1, and then condensation reagents DMAP and EDC·HCl are added under stirring (the amount of DMAP and EDC·HCl added is the equivalent of 6-amino-3-pyridylmethanol), heated to 90°C and stirred for 6 hours, and then rotary evaporated and dried to obtain;
[0074] 2. Hyperbranching reaction: Add corrosion-resistant triol and adipic acid into toluene at a molar ratio of 2-4:3-4, add p-toluenesulfonic acid under stirring (the mass of p-toluenesulfonic acid added is 1-3% of the total mass of corrosion-resistant triol and adipic acid), heat to 95°C and stir to react for 6h, rotary evaporate and dry to obtain.
[0075] Comparative Example 2
[0076] The corrosion-resistant layer is coated on the surface of the formed alloy material obtained in Example 1 (i.e., the dumbbell pin without the corrosion-resistant layer), and the coating method is as follows:
[0077] The weight parts of raw materials for the corrosion-resistant layer are stirred and mixed, stirred at room temperature for 12 hours, then filtered, sprayed on the surface of the polished, cleaned and dried formed alloy material, dried and cured to obtain the product, wherein the drying temperature is 60°C, the drying time is 30 minutes, the curing temperature is 100°C, and the curing time is 15 minutes;
[0078] The corrosion-resistant layer comprises the following raw materials in parts by weight: 50 parts of silica sol, 30 parts of methyltrimethoxysiloxane, 20 parts of deionized water, 7 parts of ethanol, and 1 part of formic acid.
[0079] The dumbbell pins obtained in Examples 1-10 and Comparative Example 2 were subjected to corrosion resistance tests (spraying the dumbbell pin surface with salt water so that the dumbbell pin surface was evenly wetted with salt water, the salt water was not acetate water, the pH was 3.1-3.3, the spraying condition was 35±2°C, the test lasted for 10 days, and the weight loss rate was measured), and the test results are shown in Table 3;
[0080] Table 3
[0081] Example 1 Example 2 Example 3 Example 3 Example 5 Weight reduction rate 10.1% 10.7% 10.4% 9.9% 10.5% Example 6 Example 7 Example 8 Example 9 Example 10 Comparative Example 2 Weight reduction rate 2.3% 2.7% 2.5% 2.2% 2.6% 6.1%
[0082] It can be seen from the data in Table 3 that the corrosion-resistant layer coated on the surface of the dumbbell pins obtained in Examples 6-10 gives the dumbbell pins good corrosion resistance, and its corrosion resistance is better than that of the dumbbell pin obtained in Comparative Example 2.
[0083] The dumbbell pins obtained in Examples 6-10 and Comparative Example 2 were subjected to an adhesion test (tested in accordance with GB / T9286. According to the standard, adhesion is divided into six levels from 0 to 5, with 0 being the best and 5 being the worst). The test results are shown in Table 4.
[0084] Table 4
[0085] Example 6 Example 7 Example 8 Example 9 Example 10 Comparative Example 2 Adhesion Level 0 Level 0 Level 0 Level 0 Level 0 Level 2
[0086] It can be seen from the data in Table 4 that the adhesion performance of the corrosion-resistant layer coated on the surface of the dumbbell pin obtained in Examples 6-10 is better than the adhesion performance of the corrosion-resistant layer coated on the surface of the dumbbell pin obtained in Comparative Example 2.
[0087] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A dumbbell pin, characterized in that: The invention comprises an alloy material and a corrosion-resistant layer coated on the surface of the alloy material, wherein the alloy material comprises the following chemical components by weight percentage: C is 0.35-0.55%; Si is 0.70-1.50%; Mn is 0.70-1.50%; Cr is 0.10-2.00%; Ni is 0.10-0.50%; Mo is 0.05-0.50%; V is 0.01-0.50%; B is 0.01-0.50%; Al is 0.020-0.050%; P is ≤0.025%; S is ≤0.015; the rest is Fe; The alloy material is prepared by the following steps: electric furnace smelting or converter smelting, refining and vacuum treatment; electroslag remelting; diffusion heat treatment; forging blanking; die forging; normalizing treatment; annealing treatment and tempering heat treatment; The process parameters of the diffusion heat treatment are: heating temperature is 1180℃~1300℃, and heat preservation is 5~15 hours; the process parameters of the forging blanking are: cooling the steel ingot after diffusion heat treatment to a temperature range of 1100℃~1250℃ for forging blanking, and the final forging temperature is ≥900℃; the process parameters of the die forging forming are: forming temperature is 950℃~1050℃; The process parameters of the normalizing treatment are: heating temperature is 900℃~920℃, holding time is 5~10 hours, after cooling, put into annealing furnace and keep at 300℃ for 5~10 hours; the process parameters of the annealing treatment are: annealing temperature is 660~680℃, holding time is 10~30 hours; the process parameters of the quenching and tempering heat treatment are: quenching temperature is 880℃~900℃, holding time is 5~10 hours, and quenching liquid or oil is used to cool to below 150℃; then tempering treatment is carried out at 400~600℃, and holding time is 10~20 hours; The corrosion-resistant layer comprises the following raw materials in parts by weight: 40-50 parts of silica sol, 20-35 parts of methyltrimethoxysiloxane, 10-30 parts of deionized water, 5-15 parts of ethanol, 5-9 parts of corrosion-resistant agent, and 0.5-1.5 parts of formic acid; The corrosion inhibitor is prepared by a hyperbranching reaction of corrosion-resistant triol and adipic acid, and the number average molecular weight of the corrosion inhibitor is 1500-2000; The corrosion-resistant triol is prepared by heating 6-amino-3-pyridylmethanol and 2,2-dihydroxymethylpropionic acid in an organic solvent DMF to 90-100° C. and reacting for 3-12 hours under the action of a condensation reagent.
2. A dumbbell pin according to claim 1, characterized in that: The molar ratio of the corrosive triol to adipic acid is 2-4:3-4.