A sheet-like porous defluorination adsorbent, preparation method and application thereof

The sheet-shaped porous rare earth-based fluorine removal adsorbent prepared by complex precipitation method solves the problems of existing fluorine removal technology in large amounts of medicines, high costs, and easy membrane pollution, and achieves efficient removal of fluorine ions, suitable for industrial wastewater and Purification of drinking water.

CN117732420BActive Publication Date: 2024-11-12WEIFU TECH (LISHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311763121.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-11-12
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

The existing fluorine removal technology has problems such as large amount of medicines, high cost, easy membrane pollution, and high energy consumption when treating fluorine-containing wastewater, and it is difficult to meet industrial emission standards and drinking water quality requirements.

Method used

The sheet-like porous rare earth-based fluorine-removing adsorbent was prepared by complex precipitation method. The complexing of lanthanum and cerium ions was stirred and precipitated under a high pH environment to form an adsorbent with a high specific surface area and a porous structure, which was used to efficiently remove fluorine ions. .

Benefits of technology

It has achieved efficient removal of fluorine ions, with a maximum adsorption capacity greater than 600mg/g, and a fluorine removal rate of more than 99.5%, adapts to the pH 3-11 range, and is suitable for industrial wastewater treatment and drinking water purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004621369490000071
    Figure BDA0004621369490000071
  • Figure BDA0004621369490000081
    Figure BDA0004621369490000081
  • Figure BDA0004621369490000091
    Figure BDA0004621369490000091
Patent Text Reader

Abstract

The present invention relates to a lamellar porous defluorination adsorbent and a preparation method thereof. The adsorbent mainly comprises two elements, cerium and lanthanum, and a lamellar porous morphology can be prepared by using a complexing agent and a precipitant together, and has a large specific surface area. The defluorination adsorbent prepared by this method is a Ce-La bimetallic oxide, and the ratio of cerium to lanthanum is 4-0.5, which can achieve complementary advantages of the defluorination ability of a single metal oxide (lanthanum oxide and cerium oxide), and can remove the solution fluoride ion concentration to a low level while having a large adsorption capacity. The preparation method of the present invention is simple, the production cost is low, the prepared adsorbent can be recycled, and the solution fluoride ion concentration after treatment is less than 1mg / L, even in the case of containing high concentrations of impurity ions, the requirements of defluorination can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sewage treatment, and in particular relates to a sheet-like porous defluorination adsorbent, a preparation method and application thereof. Background Art

[0002] Metal smelting, lithium ore purification, battery recycling, semiconductor manufacturing, photovoltaic industry, etc. will produce high-fluorine waste residue and wastewater in the process of mining fluorine-containing ores or product manufacturing. If fluorine is not removed, it will cause water pollution and reduce the purity of related products. In addition, people's requirements for fluoride ions in drinking water in life should be less than 1ppm. Long-term drinking of drinking water with fluoride ions > 1.5ppm will cause great harm to human health.

[0003] There are many methods for defluorination, such as coagulation and sedimentation, membrane treatment technology, electrocoagulation, adsorption, etc., each of which has its own advantages and disadvantages. Among them, the aluminum salt and calcium salt used in the coagulation and sedimentation method are relatively low in cost, but the amount of chemicals used in the defluorination process is large, and the residual concentration of aluminum ions and calcium ions will be high after defluorination; membrane treatment technology has good membrane selectivity, but the membrane is easily contaminated during the defluorination process and the membrane is expensive and has a limited lifespan, which is not suitable for large-scale treatment of fluoride-containing solutions; electrocoagulation method uses less chemical dosage, less sediment, and has higher efficiency, but there are problems of high energy consumption and fast electrode consumption.

[0004] Patent document number CN114214517B discloses a method of preparing dawsonite from waste lithium battery aluminum slag and further using it to remove fluorine from battery positive electrode leachate. However, this method can only reduce the fluorine ion concentration of the solution to 11ppm. If deep defluorination is not performed, not only will the 10ppm industrial emission standard not be met, but the purity of subsequent products will also be further affected. Summary of the invention

[0005] The first object of the present invention is to provide a method for preparing a rare earth-based defluorination adsorbent, which adopts a complex precipitation method, wherein lanthanum and cerium ions in the liquid phase are complexed by a complexing agent, and then precipitated under a high pH environment by stirring in a continuous stirred tank reactor to obtain a sheet-like porous defluorination adsorbent. The second object of the present invention is to provide a sheet-like rare earth-based defluorination adsorbent morphology prepared by the above-mentioned preparation method;

[0006] The third object of the present invention is to provide the use of the aforementioned rare earth-based defluorination adsorbent.

[0007] To achieve the first object of the present invention, the following technical solutions are adopted:

[0008] A method for preparing a rare earth-based defluorination adsorbent comprises adding three raw materials, namely, lanthanum, cerium salt solution and precipitant, into a continuous stirred tank reactor containing a complexing agent through a peristaltic pump to obtain a lanthanum-cerium rare earth-based defluorination adsorbent. In the preparation method of the present invention, the complexing agent preferentially complexes with metal ions, so that the crystal growth of the material at a microscopic scale is slowed down after the precipitant is added.

[0009] In one embodiment, the cerium salt comprises one or more combinations of cerium nitrate, cerium acetate, cerium sulfate and cerium chloride, the lanthanum salt is preferably one or more combinations of lanthanum nitrate, lanthanum acetate, lanthanum sulfate and lanthanum chloride, the precipitant is one or more combinations of NaOH and / or ammonia water / or sodium carbonate; the complexing agent comprises one or more combinations of citric acid, EDTA, DTPA, amino acids, phosphates and ammonia water.

[0010] To achieve the second purpose of the present invention, a complexing agent is used to preferentially complex metal ions in combination with a high stirring speed of a continuous stirred tank reactor so that the material can achieve a lamellar porous morphology, thereby increasing the specific surface area of ​​the material, improving the microscopic agglomeration of the material, and improving the adsorption performance of the adsorbent.

[0011] In order to achieve the third object of the present invention, the role of the aforementioned rare earth-based defluorination adsorbent in defluorination in sodium fluoride solution is also provided.

[0012] The beneficial effect of the present invention is to provide a flaky porous defluorination adsorbent, which comprises cerium and lanthanum elements and has a flaky porous morphology, a pore size of 2.36 to 125 nm, and a specific surface area of ​​8 to 146.42 m 2 / g. The present invention first combines the two elements of cerium and lanthanum, and combines the low-level defluorination ability of the lanthanum salt adsorbent with the large adsorption capacity of the cerium salt adsorbent to achieve complementary advantages. In addition, a special sheet-like porous structure is prepared to increase the defluorination effect of the adsorbent. Experimental results show that the sheet-like porous defluorination agent in the present invention has a high adsorption capacity, with a maximum adsorption capacity of more than 600 mg / g; the surface area is as high as 146.42 m 2 / g, the fluorine removal rate exceeds 99.5%, and the fluorine ion concentration in the solution can be reduced to 0.5ppm. It is suitable for a wide pH range, and fluorine-containing solutions with a pH of 3-11 have a fluorine removal effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0014] Figure 1It is a schematic diagram of a preparation device of a sheet-like porous defluorination adsorbent of the present invention;

[0015] Figure 2 is a SEM image of the adsorbent 1 prepared in Example 1 of the present invention;

[0016] Figure 3 This is a SEM image of the adsorbent 10 prepared in Comparative Example 4 of the present invention;

[0017] Figure 4 TEM image of the adsorbent 1 prepared in Example 1 of the present invention;

[0018] Figure 5 These are the adsorption data of the adsorbents in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2. DETAILED DESCRIPTION

[0019] The present invention provides a flaky porous defluorination adsorbent, comprising cerium and lanthanum, and having a flaky porous morphology, a pore size of 2.36 to 125 nm, and a specific surface area of ​​8 to 146.42 m 2 / g.

[0020] In the present invention, the molar ratio of the cerium element to the lanthanum element is (4-0.5):1, more preferably (2-1):1, such as 4:1, 3.5:1, 3:1, 2.5:1, 2:1, 1.5:1, 1:1, 0.5:1, preferably a range value with any of the above values ​​as the upper or lower limit.

[0021] The present invention also provides a method for preparing a sheet-like porous defluorination adsorbent, comprising the following steps:

[0022] A) introducing a cerium salt solution and a lanthanum salt solution into a mother solution containing a complexing agent and a precipitant under stirring conditions, and controlling the pH to be 8 to 12 to obtain a mixed solution;

[0023] B) aging the mixed solution under stirring conditions to obtain a sheet-like porous defluorination adsorbent.

[0024] The defluorination adsorbent prepared by the preparation method of the present invention has a specific sheet-like porous structure, which solves the problem of reduced defluorination effect caused by particle agglomeration during the preparation process of the traditional defluorination adsorbent.

[0025] In the present invention, the cerium salt is preferably one or more of cerium nitrate, cerium acetate, cerium sulfate and cerium chloride; the concentration of the cerium salt solution is preferably 0.05-0.5 mol / L, more preferably 0.1-0.4 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, preferably a range value with the above arbitrary numerical value as the upper or lower limit; the feeding rate of the cerium salt solution is preferably 1-5 mL / min, more preferably 2-4 mL / min, such as 1 mL / min, 1.5 mL / min, 2 mL / min, 2.5 mL / min, 3 mL / min, 3.5 mL / min, 4 mL / min, 4.5 mL / min, 5 mL / min, preferably a range value with the above arbitrary numerical value as the upper or lower limit.

[0026] In the present invention, the lanthanum salt is preferably one or more of lanthanum nitrate, lanthanum acetate, lanthanum sulfate and lanthanum chloride; the concentration of the lanthanum salt solution is preferably 0.05-0.5 mol / L, more preferably 0.1-0.4 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, preferably a range value with any of the above values ​​as the upper or lower limit; the feed rate of the lanthanum salt solution is preferably 1-5 mL / min, more preferably 2-4 mL / min, such as 1 mL / min, 1.5 mL / min, 2 mL / min, 2.5 mL / min, 3 mL / min, 3.5 mL / min, 4 mL / min, 4.5 mL / min, 5 mL / min, preferably a range value with any of the above values ​​as the upper or lower limit.

[0027] In the present invention, the concentration and feed rate of the lanthanum salt solution and the cerium salt solution can be regulated within the above-mentioned limited range according to the ratio of the two elements cerium and lanthanum in the product. Preferably, in one embodiment of the present invention, the feed rates of the lanthanum salt solution and the cerium salt solution are the same, and the ratio of the concentration of the cerium salt solution to the concentration of the lanthanum salt solution is 1:2, 1:1 or 2:1, that is, the molar ratio of the cerium salt to the lanthanum salt is 1:2, 1:1 or 2:1.

[0028] In the present invention, the complexing agent includes one or more of citric acid, EDTA, DTPA, amino acids, phosphates and ammonia water; the concentration of the complexing agent in the mother liquor is preferably 0.5-4 mol / L, more preferably 1-3 mol / L, such as 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, preferably a range value with any of the above values ​​as the upper or lower limit.

[0029] In the present invention, the precipitant includes one or more of NaOH, ammonia water and sodium carbonate; the concentration of the precipitant in the mother liquor is preferably 0.5-4 mol / L, more preferably 1-3 mol / L, such as 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, preferably a range value with any of the above values ​​as the upper or lower limit.

[0030] In the present invention, it is preferred to use ammonia water as both a complexing agent and a precipitating agent to prepare a flaky porous defluorinating agent. In this case, the molar ratio of the ammonia water to the total amount of the cerium salt and the lanthanum salt is preferably 1: (1-10), more preferably 1: (3-8), and most preferably 2:0.3.

[0031] The present invention preferably uses one or more of NaOH, nitric acid, hydrochloric acid and sulfuric acid to adjust the pH value, and the pH value is preferably 8 to 12, and more preferably 9 to 11. The present invention has no particular restrictions on the concentration and amount of the NaOH, nitric acid, hydrochloric acid and sulfuric acid, as long as the pH value can be adjusted to within the required range.

[0032] In the present invention, the feeding of the cerium salt solution and the lanthanum salt solution and the mixing of the mother liquor are accompanied by stirring, and the stirring speed is preferably 600-1000rad / min, more preferably 700-900rad / min, such as 600rad / min, 650rad / min, 700rad / min, 750rad / min, 800rad / min, 850rad / min, 900rad / min, 950rad / min, 1000rad / min, preferably a range value with any of the above values ​​as the upper or lower limit.

[0033] After the feeding is completed, the invention reduces the stirring speed, performs aging, and the obtained product is centrifugally washed and then dried to obtain a sheet-like porous defluorination adsorbent.

[0034] In the present invention, the stirring speed is preferably 200-500rad / min, more preferably 300-400rad / min, such as 200rad / min, 250rad / min, 300rad / min, 350rad / min, 400rad / min, 450rad / min, 500rad / min, preferably a range value with any of the above values ​​as the upper or lower limit.

[0035] In the present invention, the aging temperature is preferably 25 to 35° C., more preferably 30° C.; the aging time is 8 to 12 hours, more preferably 10 to 11 hours.

[0036] In the present invention, the drying is preferably carried out using a blast drying oven, the drying temperature is preferably 60 to 90° C., more preferably 70 to 80° C., and the drying time is preferably 12 to 30 hours, more preferably 18 to 24 hours.

[0037] The present invention also provides an application of the porous defluorination adsorbent described above in sewage defluorination. The porous defluorination adsorbent is suitable for sewage treatment environments with a pH of 3 to 11, such as industrial wastewater with a fluoride ion concentration that is too high and requires defluorination, related products with a fluoride content that is too high in the crude product and require defluorination for product purification, or when purifying water quality, the fluoride ion concentration in the water is too high to meet the drinking water standard.

[0038] The present invention provides a flaky porous defluorination adsorbent, comprising cerium and lanthanum, and having a flaky porous morphology, a pore size of 2.36 to 125 nm, and a specific surface area of ​​8 to 146.42 m 2 / g. The present invention first combines the two elements of cerium and lanthanum, and combines the low-level defluorination ability of the lanthanum salt adsorbent with the large adsorption capacity of the cerium salt adsorbent to achieve complementary advantages. In addition, a special sheet-like porous structure is prepared to increase the defluorination effect of the adsorbent. Experimental results show that the sheet-like porous defluorination agent in the present invention has a high adsorption capacity, with a maximum adsorption capacity of more than 600 mg / g; the surface area is as high as 146.42 m 2 / g, the fluorine removal rate exceeds 99.5%, and the fluorine ion concentration in the solution can be reduced to 0.5ppm. It is suitable for a wide pH range, and fluorine-containing solutions with a pH of 3-11 have a fluorine removal effect.

[0039] In order to further illustrate the present invention, a sheet-like porous defluorination adsorbent provided by the present invention, its preparation method and application are described in detail below in combination with embodiments, but it should not be understood as limiting the scope of protection of the present invention.

[0040] All the fluoride ion concentration data measured in the following experiments are based on F -The electrode (Thermo Fisher, 9609BNWP, USA) was selected and calibrated with fluoride ion standard solution (McLean 500 mg / L) diluted to 5 points (0.5 mg / -L, 1 mg / L, 2 mg / L, 5 mg / L, 10 mg / L) before use. The buffer solution preparation method during the test adopted the national standard GB7484-87 TISABII buffer solution preparation method.

[0041] Embodiment 1:

[0042] The precursor coprecipitation reactor was pre-prepared with 2 mol / L ammonia mother liquor, and 0.2 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and the control panel was used to control the peristaltic pump 3 to control the pH of the reactor at 9.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 1.

[0043] The SEM image of adsorbent 1 is shown in Figure 2 As shown in the TEM images Figure 4 As shown by Figure 2 and Figure 4 It can be seen that adsorbent 1 has a flake morphology, and the flake structure is stacked to form a porous morphology. According to the BET test, the adsorption specific surface area of ​​adsorbent 1 is 146.42 m 2 / g.

[0044] Embodiment 2:

[0045] 2 mol / L ammonia mother liquor was prepared in the precursor coprecipitation reactor in advance, and 0.1 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and then the control panel was used to control the peristaltic pump 3 to control the reactor pH at 9.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 2.

[0046] Embodiment 3:

[0047] 2 mol / L ammonia mother liquor was prepared in the precursor coprecipitation reactor in advance, 0.1 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.2 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3ml / min, and the control panel was used to control the peristaltic pump 3 to control the pH of the reactor at 9.0, and the stirring speed was 800rad / min. After the feeding was completed, the stirring speed was adjusted to 400rad / min for 10h aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24h to obtain adsorbent 3.

[0048] Comparative Example 1:

[0049] A 2 mol / L ammonia mother liquor was prepared in advance in the precursor coprecipitation reactor, and 0.2 mol of cerium (III) nitrate hexahydrate was dissolved in 1 L of deionized water. The cerium salt solution was pumped to the reactor at 3 ml / min using a peristaltic pump 1, and the pH of the reactor was controlled at 9.0 and the stirring speed was 800 rad / min using the control panel to control the peristaltic pump 3. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 4.

[0050] Comparative Example 2:

[0051] Prepare 2 mol / L ammonia mother solution in advance, dissolve 0.2 mol lanthanum (III) nitrate hexahydrate in 1L deionized water, use peristaltic pump 1 and peristaltic pump 2 to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and then use the control panel to control the peristaltic pump 3 to control the pH of the reactor at 9.0, and the stirring speed is 800 rad / min. After the feeding is completed, adjust the stirring speed to 400 rad / min for 10 hours of aging, centrifuge and wash the final product 3 times, and place it in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 5.

[0052] Test Example 1:

[0053] The adsorbents prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were used as test samples, and the adsorbent dosage of each sample was 0.2 g. 100 ml of a fluoride ion solution (prepared with sodium fluoride and deionized water) with an initial solubility of 100 mg / L was added to a glass beaker, and then 0.2 g of the adsorbent was added to each test sample. During each test, nitric acid and NaOH were used to maintain the pH at 4 during magnetic stirring at room temperature for 3 hours. After stirring, the supernatant was taken and filtered using a filter head, and the fluoride ion concentration of the filtered solution was measured. The fluoride ion removal rate was calculated based on the change in fluoride ion concentration. The results are shown in FIG. Figure 5 As shown in Table 1, Figure 5 In the figure, “Ce” corresponds to Example 1, “Ce-La11” corresponds to Example 1, “Ce-La21” corresponds to Example 2, “Ce-La11” corresponds to Example 3, and “La” corresponds to Example 2.

[0054] Table 1 Fluoride ion removal rate

[0055]

[0056] Embodiment 4:

[0057] 2 mol / L ammonia mother liquor was prepared in the precursor coprecipitation reactor in advance, and 0.2 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and then the control panel was used to control the peristaltic pump 3 to control the pH of the reactor at 8.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 6.

[0058] Embodiment 5:

[0059] The precursor coprecipitation reactor was pre-prepared with 2 mol / L ammonia mother liquor, and 0.2 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and then the control panel was used to control the peristaltic pump 3 to control the reactor pH at 10.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 7.

[0060] Embodiment 6:

[0061] The precursor coprecipitation reactor was pre-prepared with 2 mol / L ammonia mother liquor, and 0.2 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the reactor at 3 ml / min, and the control panel was used to control the peristaltic pump 3 to control the reactor pH at 11.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for 24 hours to obtain adsorbent 8.

[0062] Test Example 2:

[0063] The adsorbents in Examples 4 to 6 and Example 1 were used as test samples, and the adsorbent dosage of each sample was 0.2 g. 100 ml of fluoride ion solution (prepared by sodium fluoride and deionized water) with an initial solubility of 100 mg / L was added to a glass beaker, and then 0.2 g of the adsorbent was added to each test sample. During each test, nitric acid and NaOH were used to maintain the pH at 4 during magnetic stirring at room temperature for 3 hours. After stirring, the supernatant was filtered using a filter head, and the fluoride ion concentration of the filtered solution was measured. The fluoride ion removal rate was calculated by the change in fluoride ion concentration. The results are shown in the following table:

[0064] Table 2 Fluoride ion removal rate

[0065]

[0066] Comparative Example 3:

[0067] 2 mol / L NaOH mother liquor was prepared in the precursor coprecipitation reactor in advance, and 0.2 mol cerium (III) nitrate hexahydrate was dissolved in 1L deionized water, and 0.1 mol lanthanum (III) nitrate hexahydrate was dissolved in 1L deionized water. Peristaltic pumps 1 and 2 were used to pump the cerium salt and lanthanum salt solutions to the reactor at 3 ml / min, and then the control panel was used to control the peristaltic pump 3 to control the pH of the reactor at 9.0, and the stirring speed was 800 rad / min. After the feeding was completed, the stirring speed was adjusted to 400 rad / min for 10 hours of aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24 hours to obtain adsorbent 9.

[0068] Test Example 3:

[0069] Adsorbent 9 in Comparative Example 3 and adsorbent 1 in Example 1 were used as test samples, and the adsorbent dosage of each sample was 0.2 g. 100 ml of fluoride ion solution (prepared by sodium fluoride and deionized water) with an initial solubility of 100 mg / L was added to a glass beaker, and then 0.2 g of adsorbent was added to each test sample. Nitric acid and NaOH were used to maintain the pH at 4 during magnetic stirring for 3 hours at room temperature for each test. After stirring, the supernatant was filtered using a filter head, and the fluoride ion concentration of the filtered solution was measured. The fluoride ion removal rate was calculated by the change in the concentration of fluoride ions. The results are shown in the following table:

[0070] Table 3 Fluoride ion removal rate

[0071]

[0072] Test Example 4:

[0073] The adsorbent 1 sample adsorbed with fluoride ions was stirred in a 5M NaOH solution at a speed of 400 rpm for 0.5 h to achieve regeneration. The regenerated adsorbent was repeated with the adsorption and defluorination process described in Test Example 1. After repeating the "adsorption-regeneration" process five times, the adsorption capacity retention rate of the adsorbent for fluoride ions was still 97.26%.

[0074] Test Example 5:

[0075] The adsorption capacity of the adsorbents 4 and 5 synthesized in Comparative Examples 1 and 2 was tested, and the adsorption capacity of the defluorination adsorbent was calculated as follows:

[0076]

[0077] C0 and C e are respectively F in solution - where is the initial concentration and equilibrium concentration (mg / L), V is the solution volume (L), and m is the mass of the adsorbent (g).

[0078] 100 ml of fluoride ion solution (prepared by sodium fluoride and deionized water) with initial solubility of 100 mg / L and 1000 mg / L was added to a glass beaker, and then 0.2 g of adsorbent was added to each test sample. During each test, nitric acid and NaOH were used to maintain the pH at 4 during magnetic stirring at room temperature for 3 hours. After stirring, the supernatant was filtered using a filter head, and the fluoride ion concentration of the filtered solution was measured. The adsorption capacity of the adsorbent was calculated by the change in fluoride ion concentration. The results are shown in the following table:

[0079] Table 4 Adsorption capacity of adsorbent

[0080]

[0081] Comparative Example 4:

[0082] Instead of using a precursor coprecipitation reactor, a 500ml beaker was used as a reaction vessel, 200ml of 2mol / L NaOH was prepared in advance as a mother liquor, 0.01mol of cerium (III) nitrate hexahydrate was dissolved in 100ml of deionized water, and 0.02mol of lanthanum (III) nitrate hexahydrate was dissolved in 100ml of deionized water, and peristaltic pumps 1 and 2 were used to pump the cerium salt lanthanum salt solution to the beaker at 0.3ml / min, respectively, during which the pH was controlled at 9.0 and the stirring speed was 800rad / min. After the feeding was completed, the stirring speed was adjusted to 400rad / min for 10h aging, and the final product was centrifugally washed 3 times and placed in an 80°C forced air drying oven for drying for 24h to obtain adsorbent 10.

[0083] Test Example 6:

[0084] Adsorbent 1 in Example 1 and adsorbent 10 in Comparative Example 4 were used as test samples, and the adsorbent dosage of each sample was 0.08 g. 100 ml of fluoride ion solution (prepared by sodium fluoride and deionized water) with an initial solubility of 100 mg / L was added to a glass beaker, and then 0.08 g of adsorbent was added to each test sample. Nitric acid and NaOH were used to maintain the pH at 4 during magnetic stirring for 3 hours at room temperature for each test. After stirring, the supernatant was filtered using a filter head, and the fluoride ion concentration of the filtered solution was measured. The fluoride ion removal rate was calculated by the change in the concentration of fluoride ions. The results are shown in the following table:

[0085] Table 5 Fluoride ion removal rate

[0086]

[0087] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Application of a sheet-like porous defluorination adsorbent in defluorination of a fluorine-containing solution, and a method for preparing the sheet-like porous defluorination adsorbent, The following steps are involved: A) introducing a cerium salt solution and a lanthanum salt solution into a mother solution containing a complexing agent and a precipitant under stirring conditions, and controlling the pH to be 8 to 12 to obtain a mixed solution; Ammonia water is used as both a complexing agent and a precipitating agent, and the concentration of ammonia water in the mother liquor is 0.5-4 mol / L; the stirring speed in the step A) is 600-1000 rad / min; B) aging the mixed solution under stirring conditions to obtain a sheet-like porous defluorination adsorbent; the aging temperature is 25 to 35° C.; the aging time is 8 to 12 hours; the stirring speed in step B) is 200 to 500 rad / min; The flaky porous defluorination adsorbent comprises cerium and lanthanum elements and has a flaky porous morphology with a pore size of 2.36 to 125 nm and a specific surface area of ​​8 to 146.42 m 2 / g.

2. The use according to claim 1, It is characterized in that The molar ratio of the cerium element to the lanthanum element is (4-0.5):

1.

3. The use according to claim 1, It is characterized in that The cerium salt in the cerium salt solution includes one or more of cerium nitrate, cerium acetate, cerium sulfate and cerium chloride; the concentration of the cerium salt solution is 0.05-0.5 mol / L; The lanthanum salt in the lanthanum salt solution includes one or more of lanthanum nitrate, lanthanum acetate, lanthanum sulfate and lanthanum chloride; the concentration of the lanthanum salt solution is 0.05-0.5 mol / L.

4. The use according to claim 1, It is characterized in that The feeding rate of the lanthanum salt solution is 1 to 5 mL / min; The feeding rate of the cerium salt solution is 1-5 mL / min.