A cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnels and a preparation method thereof

By introducing cage silsesquioxane and other modifiers into the grouting material, the problem of inorganic grouting materials being difficult to pour into fine cracks in low-permeability coal tunnels is solved, and the fluidity and viscosity of the grouting material are improved. The joint strength enhances its applicability and reinforcement effect in low-permeability coal tunnels.

CN117756493BActive Publication Date: 2024-10-11CCTEG COAL MINING RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311836460.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-11
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Existing inorganic grouting materials are difficult to effectively pour into fine cracks in low-permeability coal tunnels, and water leaks out when hardened, resulting in a reduction in bonding strength and the formation of seepage channels, making it impossible to effectively reinforce.

Method used

The cage silsesquioxane modified composite grouting material is used to increase the fluidity and bonding properties and bond the interface through a mixture of octahydroxybutylated, amination and dodecylated cage silsesquioxane. Modifiers, coupling agents, accelerators and coagulants form efficient grouting materials.

Benefits of technology

It improves the fluidity and mechanical strength of the grouting material, enhances the bonding performance with the coal mass, and improves the applicability and reinforcement effect in low-permeability coal tunnels.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention proposes a cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnels and a preparation method thereof, the composite grouting material comprising the following components by mass: 80-100 parts of silicate cement clinker, 6-10 parts of reinforcing agent, 20-25 parts of cage-type silsesquioxane, 0.1-0.6 parts of interface modifier, 0.2-0.6 parts of interface coupling agent, 0.2-0.5 parts of dissolving agent, and 0.5-0.8 parts of accelerator. The present invention optimizes the formula composition of the grouting material and introduces the cage-type silsesquioxane additive, which is conducive to improving the mechanical strength of the grouting material and making it show higher compressive strength; at the same time, it can also increase the bonding strength of the grouting material and improve the applicability of the composite grouting material in low-permeability coal tunnels; and it can also improve the fluidity and injectability of the grouting material in the grouting of low-permeability coal tunnels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of grouting material preparation, and in particular, the present invention relates to a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels and a preparation method thereof. Background Art

[0002] Organic grouting materials have problems such as high price, environmental pollution, and easy aging. Inorganic grouting materials represented by ordinary cement have achieved good reinforcement effects in tunnels with simple geological conditions due to their excellent mechanical strength, environmental performance and price advantages. However, in low-permeability coal tunnels, their particle size is large, there are many coarse particles, the stability of the slurry is poor, and it is easy to precipitate water and return to concentration. It cannot be effectively injected into fine cracks and can only penetrate into tunnels with a permeability coefficient greater than 5×10 -2 cm / g coarse sand layer or cracks larger than 0.2mm, the permeability coefficient is 10 -3 -10 -4 It is difficult to penetrate into the medium-fine sand layer with a diameter of cm / g and cracks less than 0.2mm, and water is precipitated during hardening, and the solid phase volume shrinks, which reduces the bonding strength between the hardened stone and the injected matrix and forms new water seepage channels. Therefore, it is urgent to develop new high-performance composite grouting materials to improve their applicability in low-permeability coal tunnels. Summary of the invention

[0003] In view of this, the present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the present invention provides a cage-type silsesquioxane modified composite grouting material suitable for low permeability coal roadway and a preparation method thereof.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] In the first aspect, an embodiment of the present invention proposes a cage-type silsesquioxane-modified composite grouting material suitable for low permeability coal tunnels, comprising the following components in parts by weight: 80-100 parts of silicate cement clinker, 6-10 parts of a reinforcing agent, 20-25 parts of a cage-type silsesquioxane, 0.1-0.6 parts of an interface modifier, 0.2-0.6 parts of an interface coupling agent, 0.2-0.5 parts of a dissolving agent, and 0.5-0.8 parts of a coagulant.

[0006] In the embodiment of the present invention, a mixture of octahydroxybutylated cage silsesquioxane, amino cage silsesquioxane and dodecyl cage silsesquioxane is used as cage silsesquioxane and added into the grouting material. Firstly, since these substances have the advantages of smooth, dense and fine microspheres, they have a ball rolling effect in the slurry, which can reduce the internal friction between particles, expand the flow range of the slurry, and increase the flow distance of the slurry, thereby improving the fluidity and injectability of the grouting material in the grouting of low-permeability coal lanes; secondly, the cage silsesquioxane has an ideal particle gradation when used together with the grouting material, which can make the grouting material more stable during pumping. and injection process to reduce separation, sedimentation and reduce water seepage; thirdly, through the nano-size effect of the smallest silica particles such as cage-type silsesquioxane, the expansion and extension of microcracks can be constrained in the grouting material matrix, energy can be absorbed, and the stress concentration of the matrix can be reduced. Its organic active sites can increase the cross-linking degree and compatibility of the system, thereby improving the mechanical strength of the grouting material; in addition, due to the three-dimensional cage structure, multiple amino, hydroxyl, phenyl and other active groups are connected to the outside, and multiple hydrogen bonds are formed with the chemical groups on the surface of the coal body, which can increase the bonding performance of the grouting material and the coal body, thereby improving the applicability of the composite grouting material in low-permeability coal roadways.

[0007] In some embodiments, the enhancer is a mixture of Glauber's salt, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride, and the mass ratio thereof is 1:2:2:1:5.

[0008] In some embodiments, the cage silsesquioxane is a mixture of octahydroxybutylated cage silsesquioxane, aminoated cage silsesquioxane and dodecylated cage silsesquioxane, and the mass ratio thereof is (2-3):1:10, preferably 2:1:10.

[0009] In some embodiments, the interfacial modifier is a mixture of polyacrylamide, polyacrylic acid-propylene copolymer and polyvinyl butyral, and the mass ratio thereof is 2:1:(4-5), preferably 2:1:4.

[0010] In some embodiments, the interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxy silane, aminopropyl trimethoxy silane, hexadecyl trimethoxy silane and 2-hydroxyethyl methacrylate phosphate, and the mass ratio thereof is 3:1:(5-6):1, preferably 3:1:5:1.

[0011] In some embodiments, the dissolution promoter is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer, and the mass ratio thereof is 1:(2-3), preferably 1:2.

[0012] In some embodiments, the coagulant is a mixture of calcium aluminate and calcium fluoroaluminate, with a mass ratio of (2-5):1, preferably 3:1.

[0013] In a second aspect, an embodiment of the present invention further proposes a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for a low-permeability coal tunnel as described in the first aspect, comprising the following steps:

[0014] S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry;

[0015] S2, weighing the cage-type silsesquioxane, the interface modifier, the interface coupling agent, the solubilizing agent and the coagulant according to the mass fractions, adding an appropriate amount of water, stirring and mixing, and obtaining an active mixed solution;

[0016] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing, to obtain the cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0017] The preparation method of the cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels according to the embodiment of the present invention has simple process, convenient operation and low cost.

[0018] In some embodiments, in step S1, the stirring and mixing time is 10-15 minutes, preferably 10 minutes; the temperature is 15-30°C, preferably 20°C;

[0019] And / or, in step S2, the stirring and mixing time is 20-30 min, preferably 20 min; the temperature is 15-30° C., preferably 20° C.;

[0020] And / or, in step S3, the stirring and mixing time is 30-60 min, preferably 30 min; the temperature is 15-30°C, preferably 20°C. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.

[0022] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by those having ordinary skills in the field to which the present invention belongs.

[0023] Where values ​​are described herein as a range, it should be understood that such disclosure includes disclosure of all possible sub-ranges within that range, as well as specific values ​​falling within that range, regardless of whether a specific value or a specific sub-range is explicitly stated.

[0024] Herein, the words "comprises" and "includes" and variations thereof mean that other elements or integers which are permitted but not specifically described may be included.

[0025] In this article, the term "and / or" is merely a term used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent three situations: A exists alone, A and B exist at the same time, and B exists alone.

[0026] In the first aspect, the embodiment of the present invention proposes a cage-type silsesquioxane modified composite grouting material suitable for low permeability coal roadways, comprising the following components by mass: 80-100 parts of silicate cement clinker (non-limiting examples: 80 parts, 85 parts, 88 parts, 90 parts, 92 parts, 96 parts, 100 parts), 6-10 parts of reinforcing agent (non-limiting examples: 6 parts, 8 parts, 10 parts), 20-25 parts of cage-type silsesquioxane (non-limiting examples: 20 parts, 22 parts , 24 parts, 25 parts), interface modifier 0.1-0.6 parts (non-limiting examples: 0.1 parts, 0.2 parts, 0.5 parts, 0.6 parts), interface coupling agent 0.2-0.6 parts (non-limiting examples: 0.2 parts, 0.4 parts, 0.6 parts), dissolving agent 0.2-0.5 parts (non-limiting examples: 0.2 parts, 0.4 parts, 0.5 parts), coagulant 0.5-0.8 parts (non-limiting examples: 0.5 parts, 0.6 parts, 0.8 parts).

[0027] In some specific embodiments, the enhancer is a mixture of sodium sulfate, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride, and the mass ratio thereof is 1:2:2:1:5.

[0028] In some specific embodiments, the cage silsesquioxane is a mixture of octahydroxybutylated cage silsesquioxane, aminated cage silsesquioxane and dodecylated cage silsesquioxane, and the mass ratio thereof is (2-3):1:10, for example, it can be 2:1:10, 2.6:1:10, 2.8:1:10 or 3:1:10, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, the mass ratio of octahydroxybutylated cage silsesquioxane, aminated cage silsesquioxane and dodecylated cage silsesquioxane is preferably 2:1:10.

[0029] In the embodiment of the present invention, a mixture of octahydroxybutylated cage silsesquioxane, amino cage silsesquioxane and dodecyl cage silsesquioxane is used as cage silsesquioxane and added into the grouting material. Firstly, since these substances have the advantages of smooth, dense and fine microspheres, they have a ball rolling effect in the slurry, which can reduce the internal friction between particles, expand the flow range of the slurry, and increase the flow distance of the slurry, thereby improving the fluidity and injectability of the grouting material in the grouting of low-permeability coal lanes; secondly, the cage silsesquioxane has an ideal particle gradation when used together with the grouting material, which can make the grouting material more stable during pumping. and injection process to reduce separation, sedimentation and reduce water seepage; thirdly, through the nano-size effect of the smallest silica particles such as cage-type silsesquioxane, the expansion and extension of microcracks can be constrained in the grouting material matrix, energy can be absorbed, and the stress concentration of the matrix can be reduced. Its organic active sites can increase the cross-linking degree and compatibility of the system, thereby improving the mechanical strength of the grouting material; in addition, due to the three-dimensional cage structure, multiple amino, hydroxyl, phenyl and other active groups are connected to the outside, and multiple hydrogen bonds are formed with the chemical groups on the surface of the coal body, which can increase the bonding performance of the grouting material and the coal body, thereby improving the applicability of the composite grouting material in low-permeability coal roadways.

[0030] In some specific embodiments, the interfacial modifier is a mixture of polyacrylamide, polyacrylic acid-propylene copolymer and polyvinyl butyral, and the mass ratio thereof is 2:1:(4-5), for example, it can be 2:1:4, 2:1:4.2, 2:1:4.5 or 2:1:5, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, the mass ratio of polyacrylamide, polyacrylic acid-propylene copolymer and polyvinyl butyral is preferably 2:1:4.

[0031] In some specific embodiments, the interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxy silane, aminopropyl trimethoxy silane, hexadecyl trimethoxy silane and 2-hydroxyethyl methacrylate phosphate, and the mass ratio thereof is 3:1:(5-6):1, for example, it can be 3:1:5:1, 3:1:5.5:1, 3:1:5.8:1 or 3:1:6:1, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, the mass ratio of 3-isocyanate propyl trimethoxy silane, aminopropyl trimethoxy silane, hexadecyl trimethoxy silane and 2-hydroxyethyl methacrylate phosphate is preferably 3:1:5:1.

[0032] In some specific embodiments, the dissolution agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer, and the mass ratio thereof is 1:(2-3), for example, it can be 1:2, 1:2.5, 1:2.8 or 1:3, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, the mass ratio of azobenzene-glutamine copolymer to polyvinyl alcohol-polystyrene copolymer is preferably 1:2.

[0033] In some specific embodiments, the coagulant is a mixture of calcium aluminate and calcium fluoroaluminate, and the mass ratio thereof is (2-5):1, for example, it can be 2:1, 2.5:1, 3:1, 3.2:1, 3.8:1, 4:1, 4.5:1 or 5:1, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; further, the mass ratio of calcium aluminate to calcium fluoroaluminate is preferably 3:1.

[0034] In a second aspect, an embodiment of the present invention further proposes a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for a low-permeability coal tunnel as described in the first aspect, comprising the following steps:

[0035] S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry;

[0036] S2, weighing the cage-type silsesquioxane, the interface modifier, the interface coupling agent, the solubilizing agent and the coagulant according to the mass fractions, adding an appropriate amount of water, stirring and mixing, and obtaining an active mixed solution;

[0037] S3, adding the active mixed solution obtained in step S2 to the grouting base material slurry obtained in step S1, stirring and mixing, and obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0038] The preparation method of the cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels according to the embodiment of the present invention has a simple process, is easy to operate, does not require complex production equipment, has low cost, and is widely used.

[0039] In some specific embodiments, in step S1, the stirring and mixing time is 10-15 minutes, for example, it can be 10 minutes, 12 minutes, 14 minutes or 15 minutes, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 10 minutes; the temperature is 15-30°C, for example, it can be 15°C, 18°C, 20°C, 25°C or 30°C, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 20°C;

[0040] And / or, in step S2, the stirring and mixing time is 20-30 min, for example, it can be 20 min, 25 min, 28 min or 30 min, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 20 min; the temperature is 15-30°C, for example, it can be 15°C, 18°C, 20°C, 25°C, 26°C or 30°C, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 20°C;

[0041] And / or, in step S3, the stirring and mixing time is 30-60 min, for example, it can be 30 min, 35 min, 40 min, 48 min, 50 min or 60 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 30 min; the temperature is 15-30°C, for example, it can be 15°C, 18°C, 20°C, 25°C or 30°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 20°C.

[0042] The technical solution of the present invention is further described in detail below in conjunction with specific examples. Unless otherwise specified, the various raw materials used in the examples are conventional commercial products or can be prepared by known methods.

[0043] Example 1

[0044] This embodiment provides a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels, comprising the following steps:

[0045] S1, weighing 95 parts of Portland cement clinker and 8 parts of reinforcing agent according to their mass parts, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride in a mass ratio of 1:2:2:1:5;

[0046] S2, weigh 23 parts of cage-type silsesquioxane, 0.2 parts of interface modifier, 0.5 parts of interface coupling agent, 0.2 parts of dissolution promoter and 0.5 parts of coagulant according to their mass parts, add appropriate amount of water and stir and mix at 20°C for 20 minutes to obtain an active mixed solution; wherein, the cage-type silsesquioxane is a mixture of octahydroxybutylated cage-type silsesquioxane, amino-type cage-type silsesquioxane and dodecyl-type cage-type silsesquioxane in a mass ratio of 2:1:10; the interface modifier is a polypropylene in a mass ratio of 2:1:4 A mixture of olefin amide, polyacrylic acid-propylene copolymer and polyvinyl butyral; an interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxysilane, aminopropyl trimethoxysilane silane, hexadecyl trimethoxysilane and 2-hydroxyethyl methacrylate phosphate in a mass ratio of 3:1:5:1; a dissolving agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer in a mass ratio of 1:2; a coagulant is a mixture of calcium aluminate and calcium fluoroaluminate in a mass ratio of 3:1;

[0047] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing at 20° C. for 30 minutes, and thus obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0048] Example 2

[0049] This embodiment provides a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels, comprising the following steps:

[0050] S1, weighing 95 parts of Portland cement clinker and 8 parts of reinforcing agent according to their mass parts, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride in a mass ratio of 1:2:2:1:5;

[0051] S2, weigh 24 parts of cage-type silsesquioxane, 0.4 parts of interface modifier, 0.5 parts of interface coupling agent, 0.5 parts of dissolution promoter and 0.5 parts of coagulant according to their mass parts, add appropriate amount of water and stir and mix at 20°C for 30 minutes to obtain an active mixed solution; wherein, the cage-type silsesquioxane is a mixture of octahydroxybutylated cage-type silsesquioxane, amino-type cage-type silsesquioxane and dodecyl-type cage-type silsesquioxane in a mass ratio of 2:1:10; the interface modifier is a polypropylene in a mass ratio of 2:1:4 A mixture of olefin amide, polyacrylic acid-propylene copolymer and polyvinyl butyral; an interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxysilane, aminopropyl trimethoxysilane silane, hexadecyl trimethoxysilane and 2-hydroxyethyl methacrylate phosphate in a mass ratio of 3:1:5:1; a dissolving agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer in a mass ratio of 1:2; a coagulant is a mixture of calcium aluminate and calcium fluoroaluminate in a mass ratio of 3:1;

[0052] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing at 20° C. for 40 minutes, and obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0053] Example 3

[0054] This embodiment provides a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels, comprising the following steps:

[0055] S1, weighing 100 parts of Portland cement clinker and 8 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride in a mass ratio of 1:2:2:1:5;

[0056] S2, weigh 25 parts of cage-type silsesquioxane, 0.5 parts of interface modifier, 0.5 parts of interface coupling agent, 0.5 parts of dissolution promoter and 0.8 parts of coagulant according to their mass parts, add appropriate amount of water and stir and mix at 20°C for 20 minutes to obtain an active mixed solution; wherein, the cage-type silsesquioxane is a mixture of octahydroxybutylated cage-type silsesquioxane, amino cage-type silsesquioxane and dodecyl cage-type silsesquioxane in a mass ratio of 2:1:10; the interface modifier is a polypropylene in a mass ratio of 2:1:4 A mixture of olefin amide, polyacrylic acid-propylene copolymer and polyvinyl butyral; an interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxysilane, aminopropyl trimethoxysilane silane, hexadecyl trimethoxysilane and 2-hydroxyethyl methacrylate phosphate in a mass ratio of 3:1:5:1; a dissolving agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer in a mass ratio of 1:2; a coagulant is a mixture of calcium aluminate and calcium fluoroaluminate in a mass ratio of 3:1;

[0057] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing at 20° C. for 30 minutes, and thus obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0058] Example 4

[0059] This embodiment provides a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels, comprising the following steps:

[0060] S1, weighing 80 parts of Portland cement clinker and 10 parts of a reinforcing agent according to their mass fractions, adding an appropriate amount of water, stirring and mixing at 20° C. for 10 minutes, and obtaining a grouting base slurry; wherein the reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride in a mass ratio of 1:2:2:1:5;

[0061] S2, weigh 20 parts of cage-type silsesquioxane, 0.2 parts of interface modifier, 0.4 parts of interface coupling agent, 0.3 parts of dissolution promoter and 0.5 parts of coagulant according to their mass parts, add appropriate amount of water and stir and mix at 20°C for 20 minutes to obtain an active mixed solution; wherein, the cage-type silsesquioxane is a mixture of octahydroxybutylated cage-type silsesquioxane, amino-type cage-type silsesquioxane and dodecyl-type cage-type silsesquioxane in a mass ratio of 2:1:10; the interface modifier is polypropylene in a mass ratio of 2:1:4 A mixture of amide, polyacrylic acid-propylene copolymer and polyvinyl butyral; the interface coupling agent is a mixture of 3-isocyanate propyl trimethoxysilane, aminopropyl trimethoxysilane silane, hexadecyl trimethoxysilane and 2-hydroxyethyl methacrylate phosphate in a mass ratio of 3:1:5.5:1; the dissolving agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer in a mass ratio of 1:2; the coagulant is a mixture of calcium aluminate and calcium fluoroaluminate in a mass ratio of 3:1;

[0062] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing at 20° C. for 30 minutes, and thus obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0063] Example 5

[0064] This embodiment provides a method for preparing a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels, comprising the following steps:

[0065] S1, weighing 90 parts of Portland cement clinker and 6 parts of reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing at 20°C for 10 minutes to obtain a grouting base slurry; wherein the reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride in a mass ratio of 1:2:2:1:5;

[0066] S2, weigh 23 parts of cage-type silsesquioxane, 0.3 parts of interface modifier, 0.4 parts of interface coupling agent, 0.5 parts of dissolution promoter and 0.6 parts of coagulant according to their mass parts, add appropriate amount of water and stir and mix at 20°C for 20 minutes to obtain an active mixed solution; wherein, the cage-type silsesquioxane is a mixture of octahydroxybutylated cage-type silsesquioxane, amino-type cage-type silsesquioxane and dodecyl-type cage-type silsesquioxane in a mass ratio of 2:1:10; the interface modifier is a polypropylene in a mass ratio of 2:1:4 A mixture of olefin amide, polyacrylic acid-propylene copolymer and polyvinyl butyral; an interfacial coupling agent is a mixture of 3-isocyanate propyl trimethoxysilane, aminopropyl trimethoxysilane silane, hexadecyl trimethoxysilane and 2-hydroxyethyl methacrylate phosphate in a mass ratio of 3:1:5:1; a dissolving agent is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer in a mass ratio of 1:2; a coagulant is a mixture of calcium aluminate and calcium fluoroaluminate in a mass ratio of 3:1;

[0067] S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing at 20° C. for 30 minutes, and thus obtaining a cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

[0068] The compressive strength, fluidity and bonding strength of the cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnels prepared in the above embodiment were tested, and the results are shown in Table 1.

[0069] Table 1

[0070] Compressive strength / MPa Liquidity / s Bond strength / MPa Example 1 57 13 1.4 Example 2 57 16 1.3 Example 3 59 14 1.6 Example 4 53 15 1.3 Example 5 55 16 1.4

[0071] It can be seen from Table 1 that the embodiments of the present invention optimize the formula composition of the grouting material and introduce cage-type silsesquioxane additives, which is beneficial to improving the mechanical strength of the grouting material and making it exhibit higher compressive strength; at the same time, it can also increase the bonding strength of the grouting material and improve the applicability of the composite grouting material in low-permeability coal tunnels; and it can also improve the fluidity and injectability of the grouting material in grouting of low-permeability coal tunnels.

[0072] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0073] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A cage-type silsesquioxane modified composite grouting material suitable for low permeability coal roadway, It is characterized in that The invention comprises the following components in parts by weight: 80-100 parts of silicate cement clinker, 6-10 parts of reinforcing agent, 20-25 parts of cage-type silsesquioxane, 0.1-0.6 parts of interface modifier, 0.2-0.6 parts of interface coupling agent, 0.2-0.5 parts of dissolution promoter, and 0.5-0.8 parts of coagulant; The reinforcing agent is a mixture of mirabilite, gypsum, sodium fluoride, triethanolamine and hexagonal boron nitride, and the mass ratio thereof is 1:2:2:1:5; The cage silsesquioxane is a mixture of octahydroxybutylated cage silsesquioxane, aminoated cage silsesquioxane and dodecylated cage silsesquioxane, and the mass ratio thereof is (2-3):1:10; The interfacial modifier is a mixture of polyacrylamide, polyacrylic acid-propylene copolymer and polyvinyl butyral, and the mass ratio thereof is 2:1:(4-5); The interface coupling agent is a mixture of 3-isocyanate propyl trimethoxy silane, aminopropyl trimethoxy silane, hexadecyl trimethoxy silane and 2-hydroxyethyl methacrylate phosphate, and the mass ratio thereof is 3:1:(5-6):1; The dissolution promoter is a mixture of azobenzene-glutamine copolymer and polyvinyl alcohol-polystyrene copolymer, and the mass ratio thereof is 1:(2-3).

2. The cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnels according to claim 1, It is characterized in that The coagulant is a mixture of calcium aluminate and calcium fluoroaluminate, and the mass ratio thereof is (2-5):

1.

3. A method for preparing a cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnels as claimed in claim 1 or 2, It is characterized in that The steps include: S1, weighing silicate cement clinker and reinforcing agent according to their mass fractions, adding appropriate amount of water and stirring and mixing evenly to obtain grouting base material slurry; S2, weighing the cage-type silsesquioxane, the interfacial modifier, the interfacial coupling agent, the solubilizing agent and the coagulant according to their weight fractions, adding an appropriate amount of water, stirring and mixing, and obtaining an active mixed solution; S3, adding the active mixed solution obtained in step S2 to the grouting base slurry obtained in step S1, stirring and mixing, to obtain the cage-type silsesquioxane-modified composite grouting material suitable for low-permeability coal tunnels.

4. The method for preparing the cage-type silsesquioxane modified composite grouting material suitable for low-permeability coal tunnel according to claim 3, It is characterized in that In step S1, the stirring and mixing time is 10-15 minutes and the temperature is 15-30°C; And / or, in step S2, the stirring and mixing time is 20-30 minutes and the temperature is 15-30°C; And / or, in step S3, the stirring and mixing time is 30-60 minutes and the temperature is 15-30°C.