A kind of anticorrosion heat-insulating coating and its preparation method and application

By using 4-aminophenyl sodium phosphate modified carbon nitride loaded CeIn-MOF and ZnO/HNTs in the coating, the problem of difficulty in balancing anti-corrosion and thermal insulation performance in the existing technology is solved, and the excellent anti-corrosion and thermal insulation effect of the coating is achieved.

CN117757335BActive Publication Date: 2024-10-15重庆丰联科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311820738.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-10-15
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

It is difficult for the existing technology to maintain excellent thermal insulation performance while maintaining anti-corrosion capabilities, and there is a lack of effective methods that can simultaneously improve the anti-corrosion and thermal insulation properties of coatings.

Method used

The carbon nitride-loaded CeIn-MOF material modified by sodium 4-aminophenylphosphate, combined with ZnO/HNTs as the modified raw material, is added to the coating to significantly improve the anti-corrosion and thermal insulation properties.

Benefits of technology

The anti-corrosion and thermal insulation capabilities of the coating are significantly improved, forming a coating with excellent anti-corrosion and thermal insulation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004633898310000081
    Figure BDA0004633898310000081
  • Figure BDA0004633898310000082
    Figure BDA0004633898310000082
Patent Text Reader

Abstract

The present invention belongs to the technical field of coatings, and specifically relates to an anticorrosion and thermal insulation coating, and a preparation method and application thereof. CeIn-MOF@carbon nitride is obtained by modifying carbon nitride with sodium 4-aminophenylphosphate, and then loading CeIn-MOF material, and ZnO / HNTs are added to the coating as a modified raw material, which can significantly improve the anticorrosion and thermal insulation properties of the coating, that is, the anticorrosion and thermal insulation coating prepared by the present invention has excellent anticorrosion and thermal insulation properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and more specifically, relates to an anticorrosion and thermal insulation coating, and a preparation method and application thereof. Background Art

[0002] Corrosion is the process in which materials (including metals and non-metals) are damaged by surrounding media (water, air, acid, alkali, salt, solvent, etc.). Applying organic coatings on metal surfaces is a common protective measure.

[0003] Organic coatings such as epoxy resins can protect metal substrates from corrosive electrolytes by forming an effective barrier on the metal surface. Organic coatings are composed of resins, curing agents, solvents, and additives and auxiliaries such as pigments and fillers. In order to increase the service life of organic coatings, anti-corrosion fillers are usually added to their composition. Anti-corrosion fillers can improve the anti-corrosion efficiency of coatings through physical and chemical effects. Physical effects include reducing coating defects, filling organic coating pores generated during the coating curing process, enhancing the physical barrier properties of the coating, and reducing the diffusion path of corrosive molecules entering the coating / metal interface. The chemical effect is the chemical interaction between the anti-corrosion filler and the organic coating matrix, which can form new strong chemical bonds in the coating matrix, thereby changing the chemical composition of the coating, the mechanical strength of the coating to the metal substrate, and the surface hydrophobicity / hydrophilicity of the coating.

[0004] CN116285679A discloses a method for preparing a water-based epoxy-modified silicone high temperature resistant anticorrosion coating, comprising the following steps: adding acidified water to an alkoxysilane monomer for reaction to obtain a silicone prepolymer; mixing bisphenol A type epoxy resin, solvent and silicone prepolymer, heating, adding a catalyst, constant temperature reflux reaction, cooling, adding an emulsifier solution, heat preservation reaction, cooling the reaction solution to room temperature, and obtaining a water-based epoxy-modified silicone emulsion; mixing a water-based epoxy-modified silicone emulsion, deionized water, a water-based defoamer, a water-based dispersant, a water-based bentonite, a modified zinc phosphate antirust powder, wood biochar, ZIF nanosheets, glass powder, copper chrome black, barium sulfate, mica powder, film-forming aid, flash rust inhibitor, and an associative polyurethane thickener, and grinding to obtain a water-based epoxy-modified silicone high temperature resistant anticorrosion coating. The coating prepared by the present invention not only has good anticorrosion performance, but also has excellent high temperature resistance and good mechanical properties.

[0005] CN116004076A discloses a high temperature resistant, shock resistant and anti-corrosion coating and a preparation method thereof. The coating is composed of an agent A and an agent B with a mass ratio of 23:1, wherein the agent A is composed of 1020 parts of fluorene epoxy resin, 68 parts of phenolic resin, 47 parts of polyurethane resin, 13 parts of methyltrichlorosilane, 35 parts of dimethyldichlorosilane, and 37 parts of phenyltrichlorosilane; and the agent B is composed of 48 parts of dicyclohexyl phthalate, 1525 parts of a barium zinc composite metal soap stabilizer, 1020 parts of stearamide, 48 parts of benzoyl peroxide, and 610 parts of alkali-free glass fiber. The components of agent A are stirred evenly in a reactor, heated to 70-90°C, kept warm for 2.5-3.5 hours, and then cooled to obtain agent A; dicyclohexyl phthalate, composite metal soap stabilizer, and stearamide are added to the reactor, heated to 55-65°C, alkali-free glass fiber is introduced under stirring and continuously stirred, then cooled, benzoyl peroxide is added and stirred to obtain agent B. The coating provided by the present invention has good water resistance, acid resistance, alkali resistance, high strength, good seismic resistance, and good coating coverage.

[0006] CN116285577A discloses an environmentally friendly anti-corrosion coating for steel structures, which comprises the following raw materials in parts by weight: 90110 parts of epoxy resin, 1520 parts of vermiculite-loaded zinc oxide, 1020 parts of graphene / silicon dioxide / titanium dioxide composite, 1216 parts of aminosilane coupling agent, and 510 parts of curing agent; the anti-corrosion coating for steel structures of the invention uses epoxy resin as a matrix, vermiculite-loaded zinc oxide and graphene / silicon dioxide / titanium dioxide composite as inorganic fillers; and uses silane coupling agent as a cross-linking agent between the inorganic filler and the matrix to prepare an environmentally friendly anti-corrosion coating for steel structures with good heat insulation and weather resistance.

[0007] CN115595038A discloses a high-performance water-based industrial anticorrosive coating and its production process, including graphene, aluminum tripolyphosphate, zinc phosphate, water-based epoxy resin, water-based epoxy curing agent and other formulas by weight. The invention obtains the basic formula of high-performance water-based epoxy anticorrosive coating by modifying and studying the water-based epoxy curing agent system, epoxy / active hydrogen equivalent ratio, pigment filler system, and auxiliary agent system, thereby improving the comprehensive mechanical properties and corrosion resistance of the product; through the compounding test of graphene, aluminum tripolyphosphate, zinc phosphate and other fillers, a passivation film with excellent anticorrosive performance is formed on the surface of the substrate, the adhesion between the coating and the substrate and the anticorrosion ability of the coating are improved, the further corrosion of the metal substrate is prevented, and the adhesion between the coating and the substrate and the anticorrosion ability of the coating are improved; the hollow glass microspheres are coated on the surface by coprecipitation method to realize the heat insulation, heat preservation, anticorrosion and other functions of the coating.

[0008] In summary, the anti-corrosion ability or thermal insulation ability of the coating can be improved by adding additives to the coating, but there is still a technical problem to be solved in ensuring excellent thermal insulation performance while having anti-corrosion ability. Summary of the invention

[0009] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide an anti-corrosion and thermal insulation coating and its preparation method and application. CeIn-MOF@carbon nitride is obtained by modifying carbon nitride with sodium 4-aminophenylphosphate and then loading CeIn-MOF material, and ZnO / HNTs are added to the coating as the modified raw material, which can significantly improve the anti-corrosion and thermal insulation properties of the coating, that is, the anti-corrosion and thermal insulation coating prepared by the present invention has excellent anti-corrosion and thermal insulation properties.

[0010] The purpose of the invention is to provide an anti-corrosion and thermal insulation coating.

[0011] Another object of the present invention is to provide a method for preparing an anti-corrosion and thermal insulation coating.

[0012] Another object of the present invention is to provide an application of an anti-corrosion and thermal insulation coating.

[0013] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0014] An anti-corrosion and thermal insulation coating, comprising the following raw materials in parts by weight:

[0015] Epoxy resin E44 70-80 parts;

[0016] CeIn-MOF@carbon nitride 6-10 parts;

[0017] ZnO / HNTs 4-8 parts;

[0018] Silane coupling agent 8-10 parts;

[0019] Dispersant 0.5-1.5 parts;

[0020] 0.5-1.5 parts of defoaming agent;

[0021] 40-50 parts of water;

[0022] 2 to 6 parts of curing agent.

[0023] Preferably, the curing agent is diethylenetriamine or diaminodiphenyl sulfone, and the silane coupling agent is at least one of KH-550, KH-560, and KH-570.

[0024] In the present invention, further, the preparation method of CeIn-MOF@carbon nitride comprises the following steps:

[0025] (1) mechanically grinding urea and 4-aminophenylphosphonic acid sodium salt according to a certain mass ratio and mixing them uniformly, placing the obtained mixture in a crucible, and then heat-treating it in a muffle furnace to obtain modified carbon nitride;

[0026] (2) The carbon nitride, cerium salt, indium salt and terephthalic acid obtained in step (1) are ultrasonically dispersed in DMF, and then placed in an autoclave, reacted at 120-160° C. for 20-28 h, filtered, washed, and dried at 100° C. to constant weight to obtain CeIn-MOF@carbon nitride.

[0027] Preferably, in step (1), the mass ratio of urea to sodium 4-aminophenylphosphate is 1 g: 0.1-0.3 mg; the heat treatment is performed at 300-400° C. for 20-40 min, and then at 500-600° C. for 2-4 h.

[0028] Preferably, in step (2), the ratio of the carbon nitride, cerium salt, indium salt and terephthalic acid is: 50 mg: 0.1-0.3 mmol: 0.05-0.15 mmol: 0.3-0.6 mmol; the cerium salt is one of cerium nitrate, cerium chloride and cerium acetate; the indium salt is at least one of indium nitrate, indium chloride and indium acetate.

[0029] In the present invention, further, the preparation method of the ZnO / HNTs is as follows:

[0030] Halloysite nanotubes (HNTs) and zinc salt are added to deionized water, stirred evenly, and the pH is adjusted to 9-11 by a 1 mol / L sodium hydroxide solution, then stirred and reacted at 50-70°C for 1-3h, filtered, washed, dried at 60°C to constant weight, and then calcined to obtain ZnO / HNTs.

[0031] Preferably, the ratio of the HNTs to the zinc salt is 10 g: 0.2-0.6 mmol; the zinc salt is at least one of zinc nitrate, zinc chloride and zinc acetate.

[0032] Preferably, the calcination is performed at 450-550° C. for 1-3 hours.

[0033] A method for preparing the above-mentioned anti-corrosion and thermal insulation coating comprises the following steps:

[0034] CeIn-MOF@carbon nitride, ZnO / HNTs, silane coupling agent and water are placed in a high-speed mixer and mixed evenly at 45-55°C at a stirring rate of 3500-4500 r / min for 30-50 min, and then epoxy resin, dispersant and defoamer are added to obtain a mixture; finally, a curing agent is added to the above mixture and mixed evenly to obtain an anti-corrosion thermal insulation coating.

[0035] Based on the application of the above-mentioned anti-corrosion and thermal insulation coating, the anti-corrosion and thermal insulation material is used in the field of anti-corrosion and temperature resistance.

[0036] The present invention has the following beneficial effects:

[0037] (1) Modified carbon nitride is obtained by mixing 4-aminophenylphosphate sodium salt with urea and calcining the mixture, thereby increasing the active groups on the surface of the carbon nitride and improving the anti-corrosion ability of the coating;

[0038] (2) By loading CeIn-MOF onto the modified carbon nitride surface, the anti-corrosion ability of the coating is further improved.

[0039] (3) By adding silane coupling agent, the dispersion performance of the filler is improved, the interaction between the raw materials in the coating matrix is ​​enhanced, the density of the coating is enhanced, and the anti-corrosion performance of the coating is improved.

[0040] (4) The loading of zinc oxide on halloysite nanotubes promotes the uniform dispersion of zinc oxide and can significantly improve the anti-corrosion and thermal insulation properties of the coating as a whole. DETAILED DESCRIPTION

[0041] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0042] The dispersant is octadecyl dimethyl betaine; the defoamer is FoamStar A34;

[0043] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0044] Example 1

[0045] An anti-corrosion and thermal insulation coating, comprising the following raw materials in parts by weight:

[0046] Epoxy resin E44 75 parts;

[0047] CeIn-MOF@carbon nitride 8 parts;

[0048] ZnO / HNTs 6 parts;

[0049] Silane coupling agent 9 parts;

[0050] 1 part of dispersant;

[0051] 1 part of defoaming agent;

[0052] 45 parts water;

[0053] 4 parts of curing agent; the curing agent is diethylenetriamine, and the silane coupling agent is KH-560.

[0054] The preparation method of CeIn-MOF@carbon nitride comprises the following steps:

[0055] (1) 1 g of urea and 0.2 mg of 4-aminophenylphosphonic acid sodium salt were mechanically ground and mixed uniformly, and the obtained mixture was placed in a crucible, and then heat-treated at 350° C. for 30 min in a muffle furnace, and then heat-treated at 550° C. for 3 h to obtain modified carbon nitride;

[0056] (2) 50 mg of the carbon nitride obtained in step (1), 0.2 mmol of cerium nitrate, 0.1 mmol of indium chloride and 0.5 mmol of terephthalic acid were ultrasonically dispersed in 150 mL of DMF, then placed in an autoclave, reacted at 140 ° C for 24 h, filtered, washed, and dried at 100 ° C to constant weight to obtain CeIn-MOF@carbon nitride.

[0057] The preparation method of ZnO / HNTs is as follows:

[0058] 10 g of halloysite nanotubes (HNTs) and 0.4 mmol of zinc nitrate were added to 150 mL of deionized water; stirred evenly, and the pH was adjusted to 10 by a 1 mol / L sodium hydroxide solution, then stirred and reacted at 60°C for 2 h, filtered, washed, dried at 60°C to constant weight, and then calcined at 500°C for 2 h to obtain ZnO / HNTs.

[0059] A method for preparing an anticorrosive thermal insulation coating comprises the following steps:

[0060] CeIn-MOF@carbon nitride, ZnO / HNTs, silane coupling agent and water were placed in a high-speed mixer and mixed evenly at 50°C at a stirring rate of 4000r / min for 40 minutes, and then epoxy resin, dispersant and defoamer were added, and stirring was continued for 20 minutes to obtain a mixture; finally, a curing agent was added to the above mixture, and the mixture was mixed evenly to obtain an anti-corrosion and thermal insulation coating.

[0061] Example 2

[0062] An anti-corrosion and thermal insulation coating, comprising the following raw materials in parts by weight:

[0063] Epoxy resin E44 80 parts;

[0064] CeIn-MOF@carbon nitride 6 parts;

[0065] ZnO / HNTs 8 parts;

[0066] Silane coupling agent 8 parts;

[0067] 1.5 parts of dispersant;

[0068] 0.5 parts of defoaming agent;

[0069] 50 parts water;

[0070] 2 parts of curing agent; the curing agent is diaminodiphenyl sulfone, and the silane coupling agent is KH-550.

[0071] The preparation method of CeIn-MOF@carbon nitride comprises the following steps:

[0072] (1) 1 g of urea and 0.3 mg of 4-aminophenylphosphonic acid sodium salt were mechanically ground and mixed uniformly, and the obtained mixture was placed in a crucible, and then heat-treated at 400° C. for 20 min in a muffle furnace, and then heat-treated at 600° C. for 2 h to obtain modified carbon nitride;

[0073] (2) 50 mg of the carbon nitride obtained in step (1), 0.3 mmol of cerium chloride, 0.05 mmol of indium acetate and 0.6 mmol of terephthalic acid were ultrasonically dispersed in 150 mL of DMF, then placed in an autoclave, reacted at 160° C. for 20 h, filtered, washed, and dried at 100° C. to constant weight to obtain CeIn-MOF@carbon nitride.

[0074] The preparation method of ZnO / HNTs is as follows:

[0075] 10 g of halloysite nanotubes (HNTs) and 0.6 mmol of zinc chloride were added to 150 mL of deionized water, stirred evenly, and the pH was adjusted to 11 by a 1 mol / L sodium hydroxide solution, then stirred and reacted at 70 ° C for 1 h, filtered, washed, dried at 60 ° C to constant weight, and then calcined at 550 ° C for 1 h to obtain ZnO / HNTs.

[0076] A method for preparing an anticorrosive thermal insulation coating comprises the following steps:

[0077] CeIn-MOF@carbon nitride, ZnO / HNTs, silane coupling agent and water were placed in a high-speed mixer and mixed evenly at 55°C at a stirring rate of 4500r / min for 30 minutes, and then epoxy resin, dispersant and defoaming agent were added, and stirring was continued for 20 minutes to obtain a mixture; finally, a curing agent was added to the above mixture, and the mixture was mixed evenly to obtain an anti-corrosion and thermal insulation coating.

[0078] Example 3

[0079] An anti-corrosion and thermal insulation coating, comprising the following raw materials in parts by weight:

[0080] Epoxy resin E44 70 parts;

[0081] CeIn-MOF@carbon nitride 10 parts;

[0082] ZnO / HNTs 4 parts;

[0083] Silane coupling agent 10 parts;

[0084] 0.5 parts of dispersant;

[0085] 1.5 parts of defoaming agent;

[0086] 40 parts water;

[0087] 6 parts of curing agent; the curing agent is diethylenetriamine, and the silane coupling agent is KH-570.

[0088] The preparation method of CeIn-MOF@carbon nitride comprises the following steps:

[0089] (1) 1 g of urea and 0.1 mg of 4-aminophenylphosphonic acid sodium salt were mechanically ground and mixed uniformly, and the obtained mixture was placed in a crucible, and then heat-treated in a muffle furnace at 300° C. for 40 min and then at 500° C. for 4 h to obtain modified carbon nitride;

[0090] (2) 50 mg of the carbon nitride obtained in step (1), 0.1 mmol of cerium acetate, 0.15 mmol of indium nitrate and 0.3 mmol of terephthalic acid were ultrasonically dispersed in 150 mL of DMF, then placed in an autoclave, reacted at 120° C. for 28 h, filtered, washed, and dried at 100° C. to constant weight to obtain CeIn-MOF@carbon nitride.

[0091] The preparation method of ZnO / HNTs is as follows:

[0092] 10 g of halloysite nanotubes (HNTs) and 0.2 mmol of zinc acetate were added to 150 mL of deionized water, wherein the ratio of HNTs to zinc salt was 10 g:0.2 mmol; the mixture was stirred evenly, and the pH was adjusted to 9 by using a 1 mol / L sodium hydroxide solution, and then stirred at 50° C. for 3 h, filtered, washed, dried at 60° C. to constant weight, and then calcined at 450° C. for 3 h to obtain ZnO / HNTs.

[0093] A method for preparing an anticorrosive thermal insulation coating comprises the following steps:

[0094] CeIn-MOF@carbon nitride, ZnO / HNTs, silane coupling agent and water were placed in a high-speed mixer and mixed evenly at 45°C at a stirring rate of 3500r / min for 50 minutes, and then epoxy resin, dispersant and defoaming agent were added, and stirring was continued for 20 minutes to obtain a mixture; finally, a curing agent was added to the above mixture, and the mixture was mixed evenly to obtain an anti-corrosion and thermal insulation coating.

[0095] Comparative Example 1

[0096] The raw materials and preparation method of Control Example 1 are basically the same as those of Example 1, except that 14 parts of CeIn-MOF@carbon nitride are used to replace 8 parts of CeIn-MOF@carbon nitride and 6 parts of ZnO / HNTs.

[0097] Comparative Example 2

[0098] The raw materials and preparation method of Control Example 2 are basically the same as those of Example 1, except that 14 parts of ZnO / HNTs are used to replace 8 parts of CeIn-MOF@carbon nitride and 6 parts of ZnO / HNTs.

[0099] Comparative Example 3

[0100] The raw materials and preparation methods of Comparative Example 3 are basically the same as those of Example 1, except that an equal amount of carbon nitride is used to replace CeIn-MOF@carbon nitride. The preparation method of the carbon nitride is as follows:

[0101] 1 g of urea and 0.2 mg of 4-aminophenylphosphonic acid sodium salt were mechanically ground and mixed uniformly, and the obtained mixture was placed in a crucible, and then heat-treated at 350° C. for 30 min and then at 550° C. for 3 h in a muffle furnace to obtain modified carbon nitride.

[0102] Comparative Example 4

[0103] The raw materials and preparation methods of Comparative Example 4 are basically the same as those of Example 1, except that an equal amount of Ce-MOF@carbon nitride is used to replace CeIn-MOF@carbon nitride. The preparation method of Ce-MOF@carbon nitride comprises the following steps:

[0104] (1) 1 g of urea and 0.2 mg of 4-aminophenylphosphonic acid sodium salt were mechanically ground and mixed uniformly, and the obtained mixture was placed in a crucible, and then heat-treated at 350° C. for 30 min in a muffle furnace, and then heat-treated at 550° C. for 3 h to obtain modified carbon nitride;

[0105] (2) 50 mg of the carbon nitride obtained in step (1), 0.3 mmol of cerium nitrate and 0.5 mmol of terephthalic acid were ultrasonically dispersed in 150 mL of DMF, then placed in an autoclave, reacted at 140° C. for 24 h, filtered, washed, and dried at 100° C. to constant weight to obtain Ce-MOF@carbon nitride.

[0106] The thermal insulation performance of Examples 1-3 and Comparative Examples 1-2 was tested, and the test method was based on ISO22007-2. The specific test results are shown in Table 1:

[0107] Table 1:

[0108]

[0109] It can be seen from Table 1 that the coating of the present application has good thermal insulation performance.

[0110] The anticorrosion coating performance of test examples 1-3 and control examples 1-4 is specifically shown in Table 2: wherein, adhesion (pull-out adhesion): GB / T5210; impact resistance adopts GB1732; anticorrosion performance is tested according to national standards GB / T 9274-88 and GB / T 1771-91.

[0111] Table 2

[0112]

[0113] As can be seen from Table 2, the anticorrosion and thermal insulation coating prepared by the present invention has excellent corrosion resistance, and the corrosion resistance is higher than that of reference examples 1-4. Compared with Example 1, reference examples 1-2 use CeIn-MOF@ carbon nitride or ZnO / HNTs alone, which is not as good as using CeIn-MOF@ carbon nitride and ZnO / HNTs at the same time in improving corrosion resistance; compared with Example 1, reference example 3 does not add CeIn-MOF, and the anticorrosion performance and adhesion are deteriorated. Compared with Example 1, reference example 4 uses a single-component MOF compared to a two-component MOF material. The performance is significantly worse. It can be seen that the components selected in this application have a mutually reinforcing effect, so that the anticorrosion and thermal insulation material prepared by the method of the present invention has excellent thermal insulation and corrosion resistance.

[0114] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. An anticorrosion and thermal insulation coating, characterized in that: The anti-corrosion and thermal insulation coating comprises the following raw materials in parts by weight: Epoxy resin E44 70-80 parts; CeIn-MOF@carbon nitride 6-10 parts; ZnO / HNTs 4-8 parts; Silane coupling agent 8-10 parts; Dispersant 0.5-1.5 parts; 0.5-1.5 parts of defoaming agent; 40-50 parts of water; 2 to 6 parts of curing agent; The preparation method of CeIn-MOF@carbon nitride comprises the following steps: (1) mechanically grinding urea and sodium 4-aminophenylphosphate in a certain mass ratio and mixing them uniformly, placing the obtained mixture in a crucible, and then heat-treating it in a muffle furnace to obtain modified carbon nitride; the mass ratio of urea to sodium 4-aminophenylphosphate is 1g:0.1-0.3mg; (2) ultrasonically dispersing the carbon nitride, cerium salt, indium salt and terephthalic acid obtained in step (1) in DMF, then placing in an autoclave, reacting at 120-160° C. for 20-28 h, filtering, washing, and drying at 100° C. to constant weight to obtain CeIn-MOF@carbon nitride; the ratio of the carbon nitride, cerium salt, indium salt and terephthalic acid is 50 mg: 0.1-0.3 mmol: 0.05-0.15 mmol: 0.3-0.6 mmol; The preparation method of the ZnO / HNTs is as follows: Halloysite nanotubes (HNTs) and zinc salt are added to deionized water, stirred evenly, and the pH is adjusted to 9-11 by a sodium hydroxide solution with a concentration of 1 mol / L, and then stirred at 50-70°C for 1-3 hours, filtered, washed, dried at 60°C to constant weight, and then calcined to obtain ZnO / HNTs; the ratio of HNTs to zinc salt is 10g:0.2-0.6mmol.

2. The anticorrosion and thermal insulation coating according to claim 1, characterized in that: The curing agent is diethylenetriamine or diaminodiphenyl sulfone; the silane coupling agent is at least one of KH-550, KH-560 and KH-570.

3. The anticorrosion and thermal insulation coating according to claim 1, characterized in that: In step (1), the heat treatment is performed at 300-400° C. for 20-40 min, and then at 500-600° C. for 2-4 h.

4. The anticorrosion and thermal insulation coating according to claim 1, characterized in that: In step (2), the cerium salt is one of cerium nitrate, cerium chloride, and cerium acetate; and the indium salt is at least one of indium nitrate, indium chloride, and indium acetate.

5. The anticorrosion and thermal insulation coating according to claim 1, characterized in that: The zinc salt is at least one of zinc nitrate, zinc chloride and zinc acetate.

6. The anticorrosion and thermal insulation coating according to claim 1, characterized in that: The calcination is carried out at 450-550° C. for 1-3 hours.

7. A method for preparing an anticorrosive thermal insulation coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: CeIn-MOF@carbon nitride, ZnO / HNTs, silane coupling agent and water are placed in a high-speed mixer and mixed evenly at 45-55°C at a stirring rate of 3500-4500 r / min for 30-50 min, and then epoxy resin, dispersant and defoamer are added to obtain a mixture; finally, a curing agent is added to the above mixture and mixed evenly to obtain an anti-corrosion thermal insulation coating.

8. The use of an anticorrosion and thermal insulation coating according to any one of claims 1 to 6, characterized in that: The anti-corrosion and heat-insulating material is used in the field of anti-corrosion and heat-resistance.