Separation of lignocellulose components catalyzed by niobium-based single-atom catalysts in deep eutectic solvents
By using niobium-based single-atom catalyst in eutectic solvents, the problems of hemicellulose degradation and lignin structure damage caused by acid catalysis are solved, and efficient separation and high-value utilization of lignocellulose components are achieved, thereby improving the conversion Efficiency and reduce production costs.
Patent Information
- Application Number
- CN202311680417.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Prior Art In the process of component separation of lignocellulose, the use of acid catalysts leads to a lot of hemicellulose degradation and severe damage to the lignin structure, low conversion efficiency, and it is difficult to achieve efficient separation and high value of lignocellulose components. use.
Using niobium-based single atom catalyst in eutectic solvents, the niobium-based single atom catalyst is designed to catalyze the selective dissolution of lignocellulose raw materials in eutectic solvents, achieving efficient separation of lignocellulose components and using low co-consolidation. The competitive relationship between hydrogen bonds of the melt solvent and the linkage bonds of lignin at the acid site are combined with the decrystallization effect of the niobium-based single-atom catalyst to improve the enzymatic delysis efficiency of the cellulose component.
It has achieved efficient separation of various lignocellulose components, improved enzymatic efficiency of cellulose components, and the structure of lignin components is completely retained, which has reduced production costs and has good industrial application prospects.
Smart Images

Figure CN117778491B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomass chemical industry, and in particular relates to a method for separating lignocellulose components by catalyzing a niobium-based single-atom catalyst in a low eutectic solvent. Background Art
[0002] Lignocellulose is an important raw material for the preparation of bioenergy. There are usually two strategies for the preparation of bioenergy from lignocellulose: one is direct conversion, and the other is conversion after component separation. Due to the huge differences in the structure and properties of the three main components of lignocellulose (lignin, cellulose, and hemicellulose), direct conversion such as direct combustion, liquefaction, and carbonization / pyrolysis generally have problems with low conversion efficiency and complex products. After component separation and conversion, the separated components are purposefully processed into bio-based chemicals or bio-based materials according to their physical and chemical properties, which is more conducive to increasing the added value of products.
[0003] After the components are separated and then converted, the common method is to convert one or two components into water-soluble sugars or phenolic compounds. This strategy is relatively easy to implement, but the conversion efficiency is still not high. A more ideal component separation strategy is to selectively break the chemical bonds in the lignin-carbohydrate complex (LCC) to maintain the structural integrity of the three main components. Low eutectic solvents are eutectic mixtures composed of hydrogen bond acceptors (HBA) and hydrogen bond donors (HBD). During the pretreatment of biomass, low eutectic solvents selectively dissolve lignin by breaking the chemical bonds in the LCC and lignin structural units. A large number of studies have shown that in the process of separating lignocellulosic components with low eutectic solvents, the addition of acid catalysts can more effectively dissolve hemicellulose and lignin from lignocellulose, but there are generally problems of more hemicellulose degradation and serious damage to the lignin structure, which is obviously not conducive to the high-value utilization of lignocellulosic components. Summary of the invention
[0004] In view of this, the present invention aims to solve the above-mentioned problems and provides a method for separating lignocellulose components by catalyzing a niobium-based single-atom catalyst in a low eutectic solvent. By designing and synthesizing a niobium-based single-atom catalyst, the lignocellulose raw material is catalyzed to selectively dissolve in a low eutectic solvent, thereby achieving efficient separation of lignocellulose components.
[0005] The technical solution of the present invention is: a method for separating lignocellulose components catalyzed by a niobium-based single-atom catalyst in a deep eutectic solvent, and the method for separating lignocellulose components comprises the following steps:
[0006] Step 1, synthesis of niobium-based single-atom catalyst: weigh 5-20 grams of zinc nitrate and dissolve it in 275 milliliters of methanol to form solution A, weigh 0.2-2 grams of niobium oxalate and dissolve it in 25 milliliters of ethylene glycol to form solution B; mix the two solutions A and B, slowly add them to 300 milliliters of methanol containing 10-20 grams of 2-methylimidazole under vigorous stirring conditions, react at room temperature for 24 hours, then heat to 60°C and stand for 4 hours, filter; wash the filter residue with methanol, vacuum dry at 80°C for 12 hours; grind and place in a tube furnace, roast at 900°C in a nitrogen atmosphere, cool, grind and set aside;
[0007] Step 2, preparation of low eutectic solvent: weigh the hydrogen bond acceptor and hydrogen bond donor of the low eutectic solvent in a molar ratio of 1:(1-10), place in a flask, stir at 60°C for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80°C for 24 hours, and cool for use;
[0008] Step 3, separation of lignocellulose components: weighing 1.0 g of lignocellulose raw material, 5-20 g of a low eutectic solvent and 0.05-0.2 g of a catalyst, placing them in a reactor, reacting at 90-150° C. for 2-10 hours, filtering to obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0009] Step 4, lignin removal: 3 to 4 times the volume of water is added to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0010] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the low eutectic solvent for reuse;
[0011] Step 6, cellulase hydrolysis: the reaction residue of step 3 is dried in vacuum at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain the residue and filtrate; the filtrate is analyzed for sugar components;
[0012] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0013] In step 1, the heating rate of calcination in the tubular furnace is 5-10°C / min, and the temperature is raised to 900°C and then calcined for 2 hours.
[0014] In step 2, the hydrogen bond acceptor of the low eutectic solvent is one of choline chloride or betaine, and the hydrogen bond donor is one of oxalic acid, lactic acid, ethylene glycol, and urea.
[0015] In step 3, the lignocellulose raw material is one of the agricultural and forestry wastes, including corn stalks, corn cobs, wheat stalks, and bamboo and wood processing residues.
[0016] In step 6, the amount of cellulase added for enzymatic hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the enzymatic hydrolysis is performed for 72 hours.
[0017] The catalytic separation of lignocellulose components by niobium-based single-atom catalysts in deep eutectic solvents is mainly attributed to three aspects: first, the anions of the hydrogen bond acceptors of the deep eutectic solvents (Cl - ) can easily form hydrogen bonds with the hydroxyl (OH) groups of the lignocellulose polysaccharide components, and form a strong competitive relationship with the connecting bonds between the lignocellulose components, making the LCC connecting bonds unstable; secondly, the rich acid sites and excellent lignin solubility of the low eutectic solvent lead to a large number of LCC connecting bonds (mainly ester bonds and ether bonds) breaking, and lignin begins to dissolve; finally, due to its suitable acid site distribution and good catalytic de-crystallization effect on exposed cellulose, the niobium-based single-atom catalyst further breaks the connecting bonds between lignin and hemicellulose, dissolves more lignin, and further improves the enzymatic hydrolysis efficiency of the cellulose component.
[0018] Compared with the prior art, the present invention achieves the following technical effects:
[0019] 1) Utilizing low eutectic solvents and niobium-based single-atom catalysts, three goals are achieved at one stroke: efficient separation of the various components of lignocellulose, improved enzymatic hydrolysis efficiency of cellulose components, and intact retention of the structure of lignin components, which is conducive to further high-value utilization.
[0020] 2) By using low eutectic solvents and niobium-based single-atom catalysts, they can be recycled after simple filtration or distillation, which reduces production costs and has good prospects for industrial application.
[0021] 3) The catalyst has good selectivity and is easy to recover, which improves the separation efficiency of lignocellulose components in a low eutectic solvent and maintains the structural integrity of the separated components.
[0022] 4) The synergistic effect of the low eutectic solvent and the niobium-based single-atom catalyst jointly promoted the breaking of the LCC links in lignocellulose and the reduction of the crystallinity of the cellulose components, thereby achieving the efficient separation of the lignocellulose components.
[0023] 5) The separation of lignocellulose components was catalyzed by niobium-based single-atom catalysts in a low eutectic solvent. This is the first application of niobium-based single-atom catalysts in the separation of lignocellulose components. It achieved efficient removal of lignin and significantly promoted the enzymatic hydrolysis of separated cellulose. The catalyst and solvent were recycled by simple filtration or distillation, which greatly reduced the production cost and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the reaction pathway for the separation of lignocellulose components catalyzed by niobium-based single-atom catalysts in a deep eutectic solvent;
[0025] Figure 2 This is the distribution diagram of the components of corn straw separated in choline chloride-lactic acid eutectic solvent catalyzed by different acids;
[0026] Figure 3 The reuse and raw material adaptability of niobium-based single-atom catalysts and choline chloride-lactic acid low eutectic solvents. DETAILED DESCRIPTION
[0027] The following will be used to explain the implementation of the present invention in detail with examples, so that the implementation process of how the present invention applies technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations.
[0028] The percentage sign "%" involved in the present invention, unless otherwise specified, refers to mass percentage; however, the percentage of a solution, unless otherwise specified, refers to the number of grams of solute contained in 100 ml of the solution; the percentage between liquids refers to the ratio of the volumes at 20°C.
[0029] Example 1: As shown in Figure 1, corn stalk component separation
[0030] Step 1, synthesis of niobium-based single-atom catalyst: weigh 20 grams of zinc nitrate and 0.2 grams of niobium oxalate, dissolve them in 275 milliliters of methanol and 25 milliliters of ethylene glycol respectively, mix the two solutions, slowly add them to 300 milliliters of methanol containing 20 grams of 2-methylimidazole under vigorous stirring, react at room temperature for 24 hours, then heat to 60°C and stand for 4 hours, filter; wash the filter residue with methanol, vacuum dry at 80°C for 12 hours; grind and place in a tube furnace, heat to 900°C at a heating rate of 5°C / min in a nitrogen atmosphere, calcine for 2 hours, cool, grind and set aside;
[0031] Step 2, preparation of low eutectic solvent: weigh choline chloride and lactic acid in a molar ratio of 1:3, a total of 20 grams, put them in a flask, stir at 60°C for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80°C for 24 hours, and cool for use;
[0032] Step 3, separation of lignocellulose components from corn straw: weigh 1.0 g corn straw, 20 g low eutectic solvent and 0.2 g catalyst, place in a reactor, react at 120° C. for 6 hours, filter to obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0033] Step 4, lignin removal: 4 times the volume of water is added to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0034] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the low eutectic solvent for reuse;
[0035] Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours;
[0036] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0037] After measurement and calculation, the lignin yield of corn straw catalyzed by niobium-based single-atom catalyst in a choline chloride-lactic acid low eutectic solvent reached 21.9%, the cellulose yield was 62.5%, and the yields of glucose and xylose after enzymatic hydrolysis of cellulose components reached 83.0% and 56.2%, respectively.
[0038] Under the same conditions, sulfuric acid and solid acid SO4 2- / ZrO2-ATP (SZA), silicotungstic acid (STA), phosphotungstic acid (PTA), carbon nitride carrier (CN) and other single atom catalysts (copper, cobalt, molybdenum) were used to separate corn straw components. The lignin yield was lower than that of niobium-based single atom catalysts, and the glucose and xylose yields after cellulase hydrolysis were also lower than those of niobium-based single atom catalysts. Figure 2 The distribution of components separated from corn straw in a choline chloride-lactic acid eutectic solvent catalyzed by different acids is shown. It can be seen that the catalytic effect of niobium-based single atom catalyst is the best.
[0039] Example 2: Separation of corncob components
[0040] Step 1, synthesis of niobium-based single-atom catalyst: 5 g of zinc nitrate and 2 g of niobium oxalate were weighed and dissolved in 275 ml of methanol and 25 ml of ethylene glycol respectively. After the two solutions were mixed, they were slowly added to 300 ml of methanol containing 10 g of 2-methylimidazole under vigorous stirring conditions, reacted at room temperature for 24 hours, then heated to 60° C. and allowed to stand for 4 hours, and filtered; the filter residue was washed with methanol, and vacuum dried at 80° C. for 12 hours; after grinding, it was placed in a tube furnace, heated to 900° C. at a heating rate of 6° C. / min in a nitrogen atmosphere, and calcined for 2 hours, cooled, and ground for standby use;
[0041] Step 2, preparation of low eutectic solvent: weigh choline chloride and oxalic acid at a molar ratio of 1:10, a total of 20 grams, put them in a flask, stir at 60° C. for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80° C. for 24 hours, and cool it for use;
[0042] Step 3, separation of lignocellulose components from corncobs: weigh 1.0 g corncobs, 5 g low eutectic solvent and 0.05 g catalyst, place in a reactor, react at 90° C. for 10 hours, filter to obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0043] Step 4, lignin removal: add 3 times the volume of water to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0044] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the deep eutectic solvent for reuse;
[0045] Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours;
[0046] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0047] After measurement and calculation, the lignin yield of corn cobs catalyzed by niobium-based single-atom catalysts in a choline chloride-oxalic acid low eutectic solvent reached 16.2%, the cellulose yield was 54.7%, and the yields of glucose and xylose after cellulase hydrolysis reached 79.4% and 66.7%, respectively.
[0048] Example 3: Separation of wheat straw components
[0049] Step 1, synthesis of niobium-based single-atom catalyst: 10 g of zinc nitrate and 1 g of niobium oxalate were weighed and dissolved in 275 ml of methanol and 25 ml of ethylene glycol respectively. After the two solutions were mixed, they were slowly added to 300 ml of methanol containing 15 g of 2-methylimidazole under vigorous stirring conditions, reacted at room temperature for 24 hours, then heated to 60° C. and allowed to stand for 4 hours, and filtered; the filter residue was washed with methanol, vacuum dried at 80° C. for 12 hours, ground and then placed in a tube furnace, heated to 900° C. at a heating rate of 7° C. / min in a nitrogen atmosphere, and calcined for 2 hours, cooled, and ground for standby use;
[0050] Step 2, preparation of low eutectic solvent: weigh choline chloride and ethylene glycol in a molar ratio of 1:1, a total of 20 grams, put them in a flask, stir at 60° C. for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80° C. for 24 hours, and cool it for use;
[0051] Step 3, separation of wheat straw lignocellulose components: weigh 1.0 g of wheat straw, 8 g of a low eutectic solvent and 0.1 g of a catalyst, place them in a reactor, react at 150° C. for 2 hours, filter, and obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0052] Step 4, lignin removal: 3.5 times the volume of water is added to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0053] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the low eutectic solvent for reuse;
[0054] Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours;
[0055] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0056] After measurement and calculation, the lignin yield of wheat straw catalyzed by niobium-based single-atom catalyst in a choline chloride-ethylene glycol low eutectic solvent reached 20.7%, the cellulose yield was 59.4%, and the yields of glucose and xylose after cellulase hydrolysis reached 84.8% and 57.1%, respectively.
[0057] Example 4: Separation of bamboo powder components
[0058] Step 1, synthesis of niobium-based single-atom catalyst: 13 g of zinc nitrate and 0.6 g of niobium oxalate were weighed and dissolved in 275 ml of methanol and 25 ml of ethylene glycol respectively. After the two solutions were mixed, they were slowly added to 300 ml of methanol containing 12 g of 2-methylimidazole under vigorous stirring conditions, reacted at room temperature for 24 hours, then heated to 60° C. and allowed to stand for 4 hours, and filtered; the filter residue was washed with methanol, and vacuum dried at 80° C. for 12 hours; after grinding, it was placed in a tubular furnace, heated to 900° C. at a heating rate of 8° C. / min in a nitrogen atmosphere, and calcined for 2 hours, cooled, and ground for standby use;
[0059] Step 2, preparation of low eutectic solvent: weigh betaine and urea in a molar ratio of 1:5, a total of 20 grams, put them in a flask, stir at 60°C for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80°C for 24 hours, and then cool it for use;
[0060] Step 3, separation of bamboo powder lignocellulose components: weigh 1.0 g of bamboo powder, 10 g of a low eutectic solvent and 0.175 g of a catalyst, place them in a reactor, react at 100° C. for 4 hours, filter, and obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0061] Step 4, lignin removal: add 3 times the volume of water to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0062] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the low eutectic solvent for reuse;
[0063] Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours;
[0064] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0065] After measurement and calculation, the yield of lignin and cellulose components reached 24.0% and 55.5% respectively when bamboo powder was catalyzed by niobium-based single-atom catalyst in a low eutectic solvent of betaine and urea. After cellulase hydrolysis, the yields of glucose and xylose reached 74.1% and 37.6% respectively.
[0066] Example 5: Separation of Poplar Powder Components
[0067] Step 1, synthesis of niobium-based single-atom catalyst: weigh 20 g of zinc nitrate and 1.5 g of niobium oxalate, dissolve them in 275 ml of methanol and 25 ml of ethylene glycol respectively, mix the two solutions, slowly add them to 300 ml of methanol containing 18 g of 2-methylimidazole under vigorous stirring, react at room temperature for 24 hours, then heat to 60° C. and stand for 4 hours, filter; wash the filter residue with methanol, vacuum dry at 80° C. for 12 hours, grind and place in a tube furnace, heat to 900° C. at a heating rate of 10° C. / min in a nitrogen atmosphere, calcine for 2 hours, cool, grind and set aside;
[0068] Step 2, preparation of low eutectic solvent: weigh betaine and lactic acid at a molar ratio of 1:8, a total of 20 grams, put them in a flask, stir at 60° C. for 2 hours to form a uniform transparent solution; dry the transparent solution in a vacuum drying oven at 80° C. for 24 hours, and cool for standby use;
[0069] Step 3, separation of poplar wood powder lignocellulose component: weigh 1.0 g of poplar wood powder, 15 g of low eutectic solvent and 0.125 g of catalyst, place in a reactor, react at 140° C. for 8 hours, filter to obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose;
[0070] Step 4, lignin removal: 4 times the volume of water is added to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin;
[0071] Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the low eutectic solvent for reuse;
[0072] Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours;
[0073] Step 7, catalyst recovery: The filter residue of step 6 is placed at 80°C for 12 hours in vacuum drying to recover the catalyst for reuse.
[0074] After measurement and calculation, the lignin yield reached 22.4% and the cellulose yield reached 57.2% when poplar wood powder was catalyzed by niobium-based single-atom catalyst in a low eutectic solvent of betaine and lactic acid. The yields of glucose and xylose after cellulase hydrolysis reached 64.7% and 44.9%, respectively.
[0075] Figure 3 (a) shows the repeated use of niobium-based single atom catalyst and choline chloride-lactic acid low eutectic solvent. It can be seen that the separation effect of corn straw components is still good after the combination is used three times, which illustrates the good catalytic stability of niobium-based single atom catalyst and choline chloride-lactic acid low eutectic solvent.
[0076] Figure 3 (b) is the raw material adaptability of niobium-based single atom catalysts and choline chloride-lactic acid low eutectic solvents. It can be seen that the component separation effects are satisfactory whether it is corn stalks, corn cobs, wheat straw or bamboo powder, which indicates that niobium-based single atom catalysts and choline chloride-lactic acid low eutectic solvents have excellent raw material universality for the separation of lignocellulose components.
[0077] The above description describes several preferred embodiments of the present invention, but as mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. Changes and variations made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.
Claims
1. A method for separating wood cellulose components using a niobium-based single-atom catalyst in a deep eutectic solvent, characterized in that The method for separating the lignocellulose component comprises the following steps: Step 1, synthesis of niobium-based single-atom catalyst: weigh 5-20 grams of zinc nitrate and dissolve it in 275 milliliters of methanol to form solution A, weigh 0.2-2 grams of niobium oxalate and dissolve it in 25 milliliters of ethylene glycol to form solution B; mix the two solutions AB, slowly add them to 300 milliliters of methanol containing 10-20 grams of 2-methylimidazole under vigorous stirring conditions, react at room temperature for 24 hours, then heat to 60°C and stand for 4 hours, filter; wash the filter residue with methanol, vacuum dry at 80°C for 12 hours; grind and place in a tube furnace, roast at 900°C in a nitrogen atmosphere, cool, grind and set aside; Step 2, preparation of a low eutectic solvent: weigh a hydrogen bond acceptor and a hydrogen bond donor of a low eutectic solvent in a molar ratio of 1:(1-10), place them in a flask, stir at 60°C for 2 hours to form a uniform transparent solution; place the transparent solution in a vacuum drying oven at 80°C for 24 hours, and cool for standby use; the hydrogen bond acceptor of the low eutectic solvent is one of choline chloride or betaine, and the hydrogen bond donor is one of oxalic acid, lactic acid, ethylene glycol, and urea; Step 3, separation of lignocellulose components: weighing 1.0 g of lignocellulose raw material, 5-20 g of a low eutectic solvent and 0.05-0.2 g of a catalyst, placing them in a reactor, reacting at 90-150° C. for 2-10 hours, filtering to obtain a reaction filtrate and a reaction residue; the reaction filtrate is rich in lignin, and the reaction residue is rich in cellulose; the lignocellulose raw material is one of corn stalks, corn cobs, wheat stalks, and bamboo and wood processing residues in agricultural and forestry wastes; Step 4, lignin removal: 3 to 4 times the volume of water is added to the reaction filtrate of step 3, lignin is precipitated, and filtered to obtain a precipitate and a filtrate; the precipitate is rich in lignin; Step 5, solvent recovery: the filtrate of step 4 is subjected to reduced pressure distillation to recover the deep eutectic solvent for reuse; Step 6, cellulase hydrolysis: the reaction residue of step 3 is vacuum dried at 80°C for 12 hours, and then hydrolyzed by enzyme; after the hydrolysis is completed, the residue and filtrate are filtered to obtain; the filtrate is analyzed for sugar components; the amount of cellulase added for the hydrolysis is 20 FPU / g substrate, the temperature is 50°C, and the hydrolysis is carried out for 72 hours; Step 7, catalyst recovery: The filter residue of step 6 is placed at 80° C. and vacuum dried for 12 hours to recover the catalyst for reuse.
2. The method for separating lignocellulose components by catalyzing a niobium-based single-atom catalyst in a deep eutectic solvent according to claim 1, characterized in that: In step 1, the heating rate of calcination in the tubular furnace is 5-10°C / min, and the temperature is raised to 900°C and then calcined for 2 hours.