A method for growing InP thin film on gallium arsenide substrate
By alternately setting the stress buffer units of the GaxIn(1-x)P and AlxIn(1-x)P layers on the gallium arsenide substrate, the high production cost problem of InP optoelectronic devices due to high cost InP substrate materials is solved. High-quality InP film growth is achieved, reducing preparation costs and improving product performance.
Patent Information
- Application Number
- CN202211173584.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-09-26
AI Technical Summary
The existing InP optoelectronic devices rely on high-cost InP substrate materials, resulting in high production costs and it is difficult to achieve low-cost InP film preparation.
The method of growing InP films on a gallium arsenide substrate is gradually reduced by alternately setting the stress buffer units of the GaxIn(1-x)P and AlxIn(1-x)P layers on the substrate to gradually reduce the gallium and aluminum components to Relieve stress and tend to grow high-quality InP layers.
It significantly reduces the cost of InP film preparation, ensures high-quality InP layer growth, solves the stress problems caused by lattice mismatch, and improves the performance and reliability of the product.
Smart Images

Figure CN117810067B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of InP film preparation, and in particular to a method for growing an InP film on a gallium arsenide substrate. Background Art
[0002] InP optoelectronic devices have good performance and high reliability, and are widely used in optical communications and other fields. Currently, InP optoelectronic products on the market are mainly manufactured using InP substrates as substrates, but the cost of InP substrate materials is very high, resulting in high prices for InP optoelectronic devices. Therefore, how to provide a low-cost InP thin film preparation method is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0003] The object of the present invention is to provide a method for growing an InP film on a gallium arsenide substrate, which can prepare the InP film at a relatively low cost.
[0004] In order to solve the above technical problems, the present invention provides a method for growing an InP thin film on a gallium arsenide substrate, comprising:
[0005] A stress buffer layer is grown based on a gallium arsenide substrate; the stress buffer layer includes a stress buffer unit grown along a normal line, and the stress buffer unit includes at least one layer of Ga x In (1-x) P layer and at least one layer of Al x In (1-x) P layer; Ga in the stress buffer layer x In (1-x) The P layer and the Al x In (1-x) The P layers are arranged alternately, and the normal line points to a direction away from the side of the gallium arsenide substrate. x In (1-x) The gallium content decreases between the P layers. x In (1-x) The aluminum component between the P layers decreases successively. The initial value of the component x is 0.5. When the component x is 0.5, Ga x In (1-x) The P layer lattice matches the GaAs substrate layer, and there is no stress inside the GaAs substrate. x In (1-x) The P layer is lattice-matched with the GaAs substrate, and no stress is generated inside the GaAs substrate;
[0006] An InP layer is grown on the surface of the stress buffer layer facing away from the gallium arsenide substrate.
[0007] Optionally, the stress buffer unit includes an Al x In(1-x) P layer and a Ga x In (1-x) In the P layer, the initial value of the component x is 0.5.
[0008] Optionally, the stress in the stress buffer unit is balanced.
[0009] Optionally, the Ga in the same stress buffer unit x In (1-x) The gallium component of the P layer and the Al x In (1-x) The aluminum composition of the P layer is the same.
[0010] Optionally, the Ga in the same stress buffer unit x In (1-x) The doping concentration of the P layer is x In (1-x) The doping concentration of the P layer is the same as that of the Ga x In (1-x) The thickness of the P layer is related to the Al x In (1-x) The thickness of the P layer is the same.
[0011] Optionally, the growing of a stress buffer layer based on a gallium arsenide substrate includes:
[0012] Based on a gallium arsenide substrate, the stress buffer units are sequentially grown along a normal line pointing away from a side of the gallium arsenide substrate to form the stress buffer layer; after each growth of the stress buffer unit, annealing is performed, and then the next stress buffer unit is grown until the stress buffer layer is formed.
[0013] Optionally, after each stress buffer unit is grown, annealing is performed, and then the next stress buffer unit is grown until the stress buffer layer is formed, which includes:
[0014] After each stress buffer unit is grown, the introduction of the Ga source, the In source and the Al source is stopped for a preset time, and then the next stress buffer unit is grown until the stress buffer layer is formed.
[0015] Optionally, along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x) The gallium content in the P layer gradually decreases, and the Al x In (1-x) The aluminum content in the P layer gradually decreases.
[0016] Optionally, along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x)The gallium component in the P layer facing away from the GaAs substrate is x In (1-x) The gallium components in the P layer facing the gallium arsenide substrate are equal; x In (1-x) The aluminum component in the P layer facing away from the GaAs substrate is x In (1-x) The aluminum composition on the side of the P layer facing the gallium arsenide substrate is equal.
[0017] Optionally, the growing of a stress buffer layer based on a gallium arsenide substrate includes:
[0018] Growing a gallium arsenide buffer layer on the surface of the gallium arsenide substrate;
[0019] A stress buffer layer is grown on the surface of the gallium arsenide buffer layer.
[0020] The present invention provides a method for growing an InP film on a gallium arsenide substrate, comprising: growing a stress buffer layer based on the gallium arsenide substrate; the stress buffer layer comprises a stress buffer unit grown along a normal line, and the stress buffer unit comprises at least one layer of Ga x In (1-x) P layer and at least one layer of Al x In (1-x) P layer; Ga in stress buffer layer x In (1-x) P layer and Al x In (1-x) The P layers are arranged alternately, with the normal pointing away from the GaAs substrate. x In (1-x) The gallium content decreases between the P layers. x In (1-x) The aluminum content between the P layers decreases in sequence; an InP layer is grown on the surface of the stress buffer layer facing away from the gallium arsenide substrate.
[0021] Growing InP thin film on GaAs substrate can greatly reduce the cost of InP thin film preparation. x In (1-x) The P layer (x<0.5) will produce compressive stress and grow Al x In (1-x) The P layer (x<0.5) will produce tensile stress, and the Ga x In (1-x) P layer and Al x In (1-x) The P layer can balance the stress in the stress buffer layer to eliminate the stress, and then gradually reduce the Ga x In (1-x) Gallium component and Al in the P layerx In (1-x) The aluminum component in the P layer may eventually tend to grow into an InP layer, ensuring the final growth of a high-quality InP film. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions of the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 A flow chart of a method for growing an InP thin film on a gallium arsenide substrate provided by an embodiment of the present invention;
[0024] Figure 2 A flowchart of a specific method for growing an InP thin film on a gallium arsenide substrate provided by an embodiment of the present invention;
[0025] Figure 3 for Figure 2 The corresponding structural diagram. DETAILED DESCRIPTION
[0026] The core of the present invention is to provide a method for growing InP thin film on a gallium arsenide substrate. In the prior art, gallium arsenide substrate materials are mainly used to grow AlGaInP LED materials and GaInAs laser materials. Usually, a gallium arsenide buffer layer is first grown on it before the AlGaInP material and GaInAs laser material are grown. If InP is grown on a GaAs substrate, there will be a 5% lattice mismatch between it and the InP material. Therefore, during the growth process, due to the large lattice mismatch and the large stress in the epitaxial layer, the product defects are more likely to affect its performance and reliability.
[0027] The present invention provides a method for growing an InP film on a gallium arsenide substrate, comprising: growing a stress buffer layer based on the gallium arsenide substrate; the stress buffer layer comprises a stress buffer unit grown along a normal line, and the stress buffer unit comprises at least one layer of Ga x In (1-x) P layer and at least one layer of Al x In (1-x) P layer; Ga in stress buffer layer x In (1-x) P layer and Al x In (1-x) The P layers are arranged alternately, with the normal pointing away from the GaAs substrate. x In (1-x)The gallium content decreases between the P layers. x In (1-x) The aluminum content between the P layers decreases in sequence; an InP layer is grown on the surface of the stress buffer layer facing away from the gallium arsenide substrate.
[0028] Growing InP thin film on GaAs substrate can greatly reduce the cost of InP thin film preparation. x In (1-x) The P layer (x is less than 0.5) will produce compressive stress relative to the GaAs substrate, and the growth of Al x In (1-x) The P layer (x is less than 0.5) will produce tensile stress relative to the GaAs substrate, and the Ga x In (1-x) P layer and Al x In (1-x) The P layer can balance the stress in the stress buffer layer and eliminate the stress; then gradually reduce the Ga x In (1-x) Gallium component and Al in the P layer x In (1-x) The aluminum component in the P layer may eventually tend to grow into InP material. This growth method ensures the final growth of high-quality InP film.
[0029] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] Please refer to Figure 1 , Figure 1 A flow chart of a method for growing an InP thin film on a gallium arsenide substrate provided in an embodiment of the present invention.
[0031] See also Figure 1 In an embodiment of the present invention, a method for growing an InP thin film on a gallium arsenide substrate includes:
[0032] S101: growing a stress buffer layer based on a gallium arsenide substrate.
[0033] In an embodiment of the present invention, the stress buffer layer includes a stress buffer unit grown along a normal line, and the stress buffer unit includes at least one layer of Ga x In (1-x) P layer and at least one layer of Al x In (1-x) P layer; Ga in the stress buffer layerx In (1-x) The P layer and the Al x In (1-x) The P layers are arranged alternately, and the normal line points to a direction away from the side of the gallium arsenide substrate. x In (1-x) The gallium content decreases between the P layers. x In (1-x) The aluminum composition decreases successively between the P layers, and the initial value of the above-mentioned composition x is usually 0.5.
[0034] The stress buffer layer is mainly used to eliminate the stress applied to the InP layer due to lattice mismatch and other reasons when the InP layer is finally grown. The stress buffer layer specifically includes stress buffer units that grow in sequence from the surface of the GaAs substrate along the normal extension direction of the GaAs substrate surface, that is, a plurality of stress buffer units are usually grown in stacks. The stress buffer unit includes at least one layer of GaAs substrate. x In (1-x) P layer and at least one layer of Al x In (1-x) P layer. And for the entire stress buffer layer, Ga x In (1-x) P layer and Al x In (1-x) The P layers are arranged alternately. First, Ga is grown on the surface of the GaAs substrate. x In (1-x) P layer, regrowth Al x In (1-x) For example, the P layer, Ga x In (1-x) The growth of the P layer is subject to compressive stress relative to the GaAs substrate, while the Al x In (1-x) The growth of P layer is relatively x In (1-x) The P layer will be subjected to tensile stress. At this time, due to the simultaneous existence of compressive stress and tensile stress in a stress buffer unit, they can at least partially offset each other, thereby reducing or even eliminating the stress in a stress buffer unit. For the entire stress buffer layer, in the embodiment of the present invention, it is usually necessary to achieve stress balance to improve the quality of the final grown InP layer.
[0035] It should be noted that when the Ga component x = 0.5, Ga x In (1-x) The P layer is lattice-matched to the GaAs substrate, and no stress is generated inside it. When x < 0.5, Ga x In (1-x) The P layer will produce compressive stress relative to the GaAs substrate; when the Al component x = 0.5, Alx In (1-x) The P layer is lattice-matched to the GaAs substrate, and no stress is generated inside it. When x < 0.5, Al x In (1-x) P phase will produce tensile stress on the GaAs substrate. Therefore, in the embodiment of the present invention, the initial value of x is usually set to 0.5, that is, the initial value of the component x is 0.5, which is equivalent to the first layer of Ga grown on the GaAs substrate. x In (1-x) The P layer will be Ga 0.5 In 0.5 P layer, the first layer of Al grown x In (1-x) The P layer will be Al 0.5 In 0.5 Of course, the initial value of x can also be set to other values, but usually it is not much different from 0.5.
[0036] On the other hand, in the embodiment of the present invention, along the direction of the normal line pointing away from the side of the gallium arsenide substrate, the multilayer Ga x In (1-x) The gallium content decreases between the P layers. x In (1-x) The aluminum content decreases between the P layers. That is, from bottom to top, Ga x In (1-x) The gallium content in the P layer needs to be gradually reduced, and the Al x In (1-x) The aluminum component in the P layer also needs to be gradually reduced, that is, the above x value needs to be gradually reduced, usually gradually reduced to 0, at which time the InP layer can be formed. At the same time, gradually reducing the aluminum component and gallium component in each of the above film layers can avoid the occurrence of lattice mismatch caused by sudden lattice changes, reduce the stress applied to the final InP layer, and ensure the formation of a high-quality InP layer.
[0037] Specifically, this step may specifically include: growing a gallium arsenide buffer layer on the surface of the gallium arsenide substrate; and growing a stress buffer layer on the surface of the gallium arsenide buffer layer.
[0038] The above-mentioned gallium arsenide buffer layer is a conventional buffer layer grown on the surface of a gallium arsenide substrate. In the prior art, a buffer layer is usually grown first when a gallium arsenide substrate is used to eliminate stress and reduce the impact of lattice mismatch. Correspondingly, in this step, a conventional gallium arsenide buffer layer can be first grown on the surface of the gallium arsenide substrate, and then the above-mentioned stress buffer layer can be grown on the surface of the gallium arsenide buffer layer. The specific structure of the gallium arsenide buffer layer can be referred to the prior art and will not be described here. The thickness of the above-mentioned gallium arsenide buffer layer is usually 50nm to 250nm, and its doping concentration is usually 1×10 18 cm -3 Up to 1×10 19 cm -3 .
[0039] S102: growing an InP layer on the surface of the stress buffer layer facing away from the GaAs substrate.
[0040] In this step, an InP layer is grown on the surface of the stress buffer layer facing away from the GaAs substrate to complete the growth preparation of the InP film. x In (1-x) Gallium component and Al in the P layer x In (1-x) The process of reducing the aluminum content in the P layer to 0. In the embodiment of the present invention, the total thickness of the stress buffer layer is usually 50nm to 500nm, and the thickness of the InP layer is usually 100nm to 500nm.
[0041] A method for growing an InP thin film on a gallium arsenide substrate provided by an embodiment of the present invention can greatly reduce the cost of preparing the InP thin film by using gallium arsenide as a substrate to grow the InP thin film. x In (1-x) The P layer (x is less than 0.5) will produce compressive stress relative to the GaAs substrate, and the growth of Al x In (1-x) The P layer (x is less than 0.5) will produce tensile stress relative to the GaAs substrate, and the Ga x In (1-x) P layer and Al x In (1-x) The P layer can balance the stress in the stress buffer layer and eliminate the stress; then gradually reduce the Ga x In (1-x) Gallium component and Al in the P layer x In (1-x) The aluminum component in the P layer can eventually grow toward an InP layer, ensuring the final growth of a high-quality InP film.
[0042] The specific contents of the method for growing an InP thin film on a gallium arsenide substrate provided by the present invention will be described in detail in the following invention embodiments.
[0043] Please refer to Figure 2 as well as Figure 3 , Figure 2 A flowchart of a specific method for growing an InP thin film on a gallium arsenide substrate provided by an embodiment of the present invention; Figure 3 for Figure 2 The corresponding structural diagram.
[0044] See also Figure 2 as well as Figure 3 In an embodiment of the present invention, a method for growing an InP thin film on a gallium arsenide substrate includes:
[0045] S201: Based on the gallium arsenide substrate, stress buffer units are sequentially grown along a normal line pointing away from a side of the gallium arsenide substrate to form a stress buffer layer.
[0046] After each stress buffer unit is grown, annealing is performed, and then the next stress buffer unit is grown until the stress buffer layer is formed.
[0047] In the embodiment of the present invention, the stress buffer unit includes an Al x In (1-x) P layer and a Ga x In (1-x) P layer. That is, in the embodiment of the present invention, an adjacent layer of Al x In (1-x) P layer and Ga x In (1-x) The P layer is used as a stress buffer unit to design the entire stress buffer layer. Specifically, in the embodiment of the present invention, it is necessary to form a stress balance in a single stress buffer unit, that is, the Al x In (1-x) P layer and Ga x In (1-x) The P layer needs stress balance. Of course, in the embodiment of the present invention, multiple stress buffer units can also be arranged to compensate each other to achieve stress balance of the stress buffer layer, but its design and implementation process are relatively complicated.
[0048] When the stress in a single stress buffer unit is balanced, in the embodiment of the present invention, it is usually necessary to make the Ga x In (1-x) The gallium component of the P layer and the Al x In (1-x)The aluminum component of the P layer is the same. That is, the value of x in the same stress buffer unit is equal. For example, if the specific aluminum component of the same stress buffer unit is Ga 0.5 In 0.5 P layer, the other film layer is Al 0.5 In 0.5 P layer. Correspondingly, the Ga x In (1-x) The doping concentration of the P layer is x In (1-x) The doping concentration of the P layer is the same as that of the Ga x In (1-x) The thickness of the P layer is related to the Al x In (1-x) The thickness of the P layer is the same. At this time, it can be ensured that the Ga x In (1-x) P layer and Al x In (1-x) The P layers are substantially the same, and the stresses generated therein are also substantially the same, so that stress balance can be achieved in a single stress buffer unit.
[0049] Specifically, in this step, based on the structure of the stress buffer unit, each stress buffer unit is grown in sequence along the normal line pointing away from the side of the gallium arsenide substrate, and annealing is performed after each stress buffer unit is grown, so that the formed stress buffer unit is specifically formed and part of the stress is released; then the next stress buffer unit is grown until the stress buffer layer. That is, in the embodiment of the present invention, each stress buffer unit is gradually formed from bottom to top, and different stress buffer units are Ga x In (1-x) The gallium content in the P layer gradually decreases, and the Al x In (1-x) The aluminum content in the P layer gradually decreases.
[0050] Specifically, in this step, after each stress buffer unit is grown, the introduction of Ga source, In source and Al source is stopped for a preset time, and then the next stress buffer unit is grown until the stress buffer layer is formed. That is, in this step, the formation of the stress buffer unit is terminated by stopping the introduction of reactants, specifically stopping the introduction of Ga source, In source and Al source. Stop for a preset time, usually after stopping for 5 to 30 seconds, and then continue the preparation of the next stress buffer unit. The above-mentioned process of stopping the introduction of Ga source, In source and Al source for a preset time is the annealing process. In this step, annealing for 5 to 30 seconds after the growth of the stress buffer unit can achieve the purpose of stress balance and stress elimination. Through the growth method of layer-by-layer growth and annealing, the InP film can be better grown on the gallium arsenide substrate.
[0051] Specifically, in the embodiment of the present invention, along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x) The gallium content in the P layer gradually decreases, and the Al x In (1-x) The aluminum content in the P layer gradually decreases. That is, in the same film layer, the Ga x In (1-x) The Ga content in the P layer gradually decreases, while the Al x In (1-x) The Al content in the P layer also gradually decreases. That is, the distribution of Ga and Al in the same film layer is not equal everywhere. Specifically, along the thickness direction, Ga x In (1-x) The Ga content on the side of the P layer close to the GaAs substrate is higher than the Ga content on the side away from the GaAs substrate. x In (1-x) The Al content of the P layer close to the GaAs substrate is higher than that of the P layer far from the GaAs substrate. The above structure can make the distribution of Ga and Al in the stress buffer layer more uniform, thereby further reducing the stress between different film layers.
[0052] Specifically, in an embodiment of the present invention, along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x) The gallium component in the P layer facing away from the gallium arsenide substrate is x In (1-x) The gallium components in the P layer facing the gallium arsenide substrate are equal; x In (1-x) The aluminum component in the P layer facing away from the GaAs substrate is x In (1-x) The aluminum composition on the side of the P layer facing the gallium arsenide substrate is equal.
[0053] That is, when growing a layer of Ga x In (1-x) P layer, the Ga x In (1-x) The composition of Ga at the final moment of P layer growth is related to the growth of the next layer of Ga x In (1-x) The Ga component is the same at the initial moment when the P layer is formed, that is, along the normal line pointing away from the GaAs substrate, Ga x In (1-x) The gallium component on the side of the P layer facing away from the GaAs substrate is different from the adjacent Ga x In (1-x)The gallium composition on the side of the P layer facing the GaAs substrate is equal; accordingly, when growing a layer of Al x In (1-x) P layer, the Al x In (1-x) The composition of Al at the final moment of P layer growth is related to the growth of the next layer of Al x In (1-x) The Al composition is the same at the initial moment when the P layer is formed, that is, along the normal line pointing away from the GaAs substrate, Al x In (1-x) The Al composition on the side of the P layer facing away from the GaAs substrate is different from the adjacent Al x In (1-x) The Al composition in the P layer facing the GaAs substrate is equal. x In (1-x) The Ga composition in the P layer is 0.5, and the Ga x In (1-x) The Ga component in the P layer is 0.4. 0.5 In 0.5 In the P layer, the Ga composition at the initial growth stage, i.e., the side close to the GaAs substrate, is 0.5, while at the final growth stage, i.e., the Ga composition at the side away from the GaAs substrate, needs to be reduced to 0.4. The above structure can minimize the stress caused by the different Ga and Al compositions between the stress buffer units.
[0054] Specifically, in the embodiment of the present invention, the above-mentioned Ga x In (1-x) The thickness of the P layer is usually between 5nm and 20nm, and the doping concentration is usually between 1×10 18 cm -3 Up to 1×10 19 cm -3 ; The corresponding Al x In (1-x) The thickness of the P layer is usually between 5nm and 20nm, and the doping concentration is usually between 1×10 18 cm -3 Up to 1×10 19 cm -3 .
[0055] S202: growing an InP layer on the surface of the stress buffer layer facing away from the GaAs substrate.
[0056] This step is basically the same as S102 in the above-mentioned embodiment of the invention. Please refer to the above-mentioned embodiment of the invention for the content, and no further description will be given here.
[0057] The method for growing an InP film on a gallium arsenide substrate provided by the embodiment of the present invention enables the stress buffer unit itself to achieve stress balance, and effectively reduces the stress between adjacent stress buffer units, so that the entire stress buffer layer is in a stress balance state, and the quality of the final InP film is improved as much as possible. The above-mentioned growth method has small internal stress in the epitaxial layer and good crystal quality, which solves the problem that InP optoelectronic devices were mainly grown on InP substrates but were expensive in the past. Growing high-quality InP materials on GaAs substrates can reduce the substrate cost by more than 90%.
[0058] Three specific InP film preparation methods are provided below, and the resulting InP films are compared and introduced.
[0059] The first step is to place the GaAs substrate into MOCVD (metal organic chemical vapor deposition) and raise the temperature to 700 degrees Celsius to grow a 200nm GaAs buffer layer with a doping concentration of 5×10 18 cm -3 .
[0060] Step 2: Grow 10nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , and then grow 10nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x1 to x2 at a uniform speed, where x1=0.5 and x2=0.45.
[0061] Step 3: Stop supplying Ga source, In source and Al source for 15 seconds.
[0062] Step 4: Grow 10nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , and then grow 10nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x2 to x3 at a uniform speed, where x3=0.4.
[0063] Step 5: Stop supplying Ga source, In source and Al source for 15 seconds.
[0064] Step 6: Grow 10nm thick Ga x In (1-x) P layer, doping concentration is 5×1018 cm -3 , and then grow 10nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x3 to x4 at a uniform speed, where x4=0.35.
[0065] Step 7. Stop supplying Ga source, In source and Al source for 15 seconds.
[0066] Step 8: Using a growth method similar to steps 4 to 5, the component x is reduced to grow 10nm Ga x In (1-x) P layer, and grow 10nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x(n-1) to xn at a uniform speed, where x(n-1)>xn, xn=0, that is, x11=0, for a total of 10 cycles.
[0067] Step 9: Stop the introduction of Ga source, In source, and Al source for 15 seconds; at this time, the Ga x In (1-x) P layer and Al x In (1-x) The total thickness of the P layer is 200 nm.
[0068] Step 10: Grow a 300nm InP layer.
[0069] The wafer grown in the above steps was taken out from MOCVD, and the total number of defects was detected by defect scanning equipment, which was 305. The surface was flat and had good morphology under a microscope. XRD (X-ray diffraction) was used to scan the 004 surface ω-2θ, and the half-peak width of the InP layer was 120 arcsec. The microscope and XRD test results showed that the grown InP material crystals had good quality.
[0070] The second method is to place the GaAs substrate in MOCVD and raise the temperature to 700 degrees Celsius to grow a 200nm GaAs buffer layer with a doping concentration of 5×10 18 cm -3 .
[0071] Step 2: Grow 15nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , and then grow 15nm thick Al x In (1-x)P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x1 to x2 at a uniform speed, where x1=0.5 and x2=0.45.
[0072] Step 3: Stop supplying Ga source, In source and Al source for 15 seconds.
[0073] Step 4: Grow 15nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , and then grow 15nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x2 to x3 at a uniform speed, where x3=0.4.
[0074] Step 5: Stop supplying Ga source, In source and Al source for 15 seconds.
[0075] Step 6: Grow 15nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , and then grow 15nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x3 to x4 at a uniform speed, where x4=0.35.
[0076] Step 7. Stop supplying Ga source, In source and Al source for 15 seconds.
[0077] Step 8: Using a growth method similar to steps 4 to 5, the component x is reduced to grow 15nm Ga x In (1-x) P layer, and grow 15nm thick Al x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x gradually decreases from x(n-1) to xn at a uniform speed, where x(n-1)>xn, xn=0, that is, x11=0, for a total of 10 cycles.
[0078] Step 9: Stop the introduction of Ga source, In source, and Al source for 15 seconds; at this time, the Ga x In (1-x) P layer and Al x In (1-x)The total thickness of the P layer is 300 nm.
[0079] Step 10: Grow a 300nm InP layer.
[0080] The wafer grown in the above steps was taken out from MOCVD, and the total number of defects was detected by defect scanning equipment, which was 325. The surface was flat and the morphology was good under a microscope. XRD (X-ray diffraction) was used to scan the 004 surface ω-2θ, and the half-peak width of the InP layer was 140 arcsec. The microscope and XRD test results showed that the grown InP material crystals had good quality.
[0081] The third type is prepared in a conventional manner in the prior art without using a direct transition growth scheme of the above-mentioned technology.
[0082] The first step is to place the GaAs substrate into the MOCVD, raise the temperature to 700 degrees Celsius, and grow a 200nm GaAs buffer layer with a doping concentration of 5×10 18 cm -3 .
[0083] Step 2: Grow 300nm thick Ga x In (1-x) P layer, doping concentration is 5×10 18 cm -3 , where x decreases gradually and uniformly from 0.5 to 0.
[0084] The third step is to grow a 300nm InP layer.
[0085] The grown wafer was taken out from MOCVD, and the total number of defects detected by defect scanning equipment was 86750. The surface was rough with many pits under a microscope. XRD was used to scan the 004 surface ω-2θ, and the half-peak width of the InP layer was 720arcsec. The microscope and XRD test results showed that the quality of the grown InP material crystal was very poor.
[0086] In a comprehensive comparison, the quality of the InP layer grown by the first two preparation methods is much better than that of the InP layer grown by the third preparation method. The comparison results are shown in Table 1 below.
[0087] Table 1. Comparison results
[0088]
[0089] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0090] Professionals may further appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, computer software, or a combination of the two. In order to clearly illustrate the interchangeability of hardware and software, the composition and steps of each example have been generally described in the above description according to function. Whether these functions are performed in hardware or software depends on the specific application and design constraints of the technical solution. Professionals and technicians may use different methods to implement the described functions for each specific application, but such implementation should not be considered to be beyond the scope of the present invention.
[0091] The steps of the method or algorithm described in conjunction with the embodiments disclosed herein may be implemented directly using hardware, a software module executed by a processor, or a combination of the two. The software module may be placed in a random access memory (RAM), a memory, a read-only memory (ROM), an electrically programmable ROM, an electrically erasable programmable ROM, a register, a hard disk, a removable disk, a CD-ROM, or any other form of storage medium known in the art.
[0092] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0093] The above is a detailed introduction to a method for growing an InP thin film on a gallium arsenide substrate provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for growing an InP thin film on a gallium arsenide substrate, It is characterized in that include: A stress buffer layer is grown based on a gallium arsenide substrate; the stress buffer layer includes a stress buffer unit grown along a normal line, and the stress buffer unit includes at least one layer of Al x In (1-x) P layer and at least one layer of Ga x In (1-x) P layer; the Al in the stress buffer layer x In (1-x) The P layer and the Ga x In (1-x) The P layers are arranged alternately, and along the normal line, point to a direction away from the gallium arsenide substrate. x In (1-x) The aluminum content decreases between the P layers. x In (1-x) The gallium content decreases successively between the P layers; Growing an InP layer on the surface of the stress buffer layer facing away from the gallium arsenide substrate; The stress buffer unit includes an Al x In (1-x) P layer and a Ga x In (1-x) P layer, the initial value of component x is 0.5; The Ga in the same stress buffer unit x In (1-x) The gallium component of the P layer and the Al x In (1-x) The aluminum composition of the P layer is the same; The Ga in the same stress buffer unit x In (1-x) The doping concentration of the P layer is x In (1-x) The doping concentration of the P layer is the same as that of the Ga x In (1-x) The thickness of the P layer is related to the Al x In (1-x) The thickness of the P layer is the same; The method of growing a stress buffer layer based on a gallium arsenide substrate comprises: Based on the gallium arsenide substrate, the stress buffer units are sequentially grown along a normal line pointing away from the gallium arsenide substrate to form the stress buffer layer; after each growth of the stress buffer unit, annealing is performed, and then the next stress buffer unit is grown until the stress buffer layer is formed; Along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x) The gallium content in the P layer gradually decreases, and the Al x In (1-x) The aluminum content in the P layer gradually decreases; Along the normal line pointing away from the gallium arsenide substrate, the Ga x In (1-x) The gallium component in the P layer facing away from the GaAs substrate is x In (1-x) The gallium components in the P layer facing the gallium arsenide substrate are equal; x In (1-x) The aluminum component in the P layer facing away from the GaAs substrate is x In (1-x) The aluminum composition on the side of the P layer facing the gallium arsenide substrate is equal.
2. The method according to claim 1, It is characterized in that After each stress buffer unit is grown, annealing is performed, and then the next stress buffer unit is grown until the stress buffer layer is formed, which comprises: After each stress buffer unit is grown, the introduction of the Ga source, the In source and the Al source is stopped for a preset time, and then the next stress buffer unit is grown until the stress buffer layer is formed.
3. The method according to claim 1, It is characterized in that The method of growing a stress buffer layer based on a gallium arsenide substrate comprises: Growing a gallium arsenide buffer layer on the surface of the gallium arsenide substrate; A stress buffer layer is grown on the surface of the gallium arsenide buffer layer.