A method for extracting lithium from carbonate salt lakes using an adsorption-coupled salt gradient solar pool

By using lithium ion adsorbent to adsorb and desorption of salt lake brine in salt gradient solar cell technology, the problem of large land occupation and long periods in traditional technology is solved, and the concentration of lithium ion and precipitation amount and rate of lithium carbonate are improved. It achieves efficient and clean lithium ion extraction effect.

CN117886340BActive Publication Date: 2024-11-26INST OF MINERAL RESOURCES CHINESE ACAD OF GEOLOGICAL SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410065036.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-11-26
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

Traditional salt gradient solar pool technology occupies a large area of ​​land, has a long process cycle, and the lithium ion enrichment effect is unstable, making it difficult to adapt to the needs of the fragile ecological environment of the plateau.

Method used

Lithium ion adsorbent is used to adsorb and desorb the raw material brine of carbonate-type salt lakes. After evaporation and concentration, the enriched lithium ion liquid is injected into the solar cell as a hydroxide, thereby achieving efficient enrichment of lithium ions and crystallization of lithium carbonate.

Benefits of technology

The concentration of lithium ions, the precipitation amount and crystallization rate of lithium carbonate are significantly improved, the impact on land use and climate is reduced, and clean production and efficient lithium extraction are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117886340B_ABST
    Figure CN117886340B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of hydrometallurgy, and relates to a method for extracting lithium from a carbonate salt lake by an adsorption-coupled salt gradient solar pool, comprising the following steps: loading a lithium ion adsorbent into a column, introducing carbonate salt lake raw brine into the adsorption column until adsorption is saturated, then introducing dilute hydrochloric acid to elute through the column, and collecting a desorption solution rich in lithium ions; the desorption solution is evaporated and concentrated to further increase the concentration of lithium ions in the solution, and then the solution enriched with lithium ions is introduced into the lower troposphere of the solar pool as a brine for crystallization of lithium carbonate, and lithium carbonate is collected. The present invention uses a high-concentration lithium ion solution enriched with a fiber-based adsorption material as brine to directly inject it into the lower troposphere of a salt gradient solar pool, couples adsorption with a salt gradient solar pool technology, and increases the amount of lithium carbonate precipitation by 22.73% and the crystallization rate of lithium carbonate by 50% compared with a traditional salt gradient solar pool process, greatly improving the efficiency and yield of lithium extraction in a traditional salt gradient solar pool.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for extracting lithium from a carbonate salt lake, and in particular to a method for efficiently extracting lithium from a carbonate salt lake by using an adsorption-coupled salt gradient solar pond, and belongs to the technical field of hydrometallurgy. Background Art

[0002] The salt gradient solar pool lithium extraction technology is a simple lithium extraction salt field structure designed according to the brine concentration law, which is divided into two parts: evaporation and crystallization. The evaporation system is equipped with multiple drying pools. The first evaporation pool is both a pre-drying pool and a raw brine storage pool; the second evaporation pool is a secondary drying pool; the third evaporation pool is the main drying pool, which consists of several independent small pools; the last level, the fourth evaporation pool, is both a drying pool and a brine storage pool; a pump station is set between the third and fourth drying pools to ensure the timely use of brine. The raw brine is pre-dried through multiple stages to increase the lithium ion concentration in the brine, meet the crystallization requirements, and is made into irrigation brine (the lithium ion concentration in the irrigation brine is 1.5-1.9g / L in summer and 1.8-2.1g / L in winter) and injected into the salt gradient solar pool for lithium carbonate crystallization.

[0003] The salt gradient solar pond consists of three parts: the upper troposphere, the non-troposphere (also known as the salinity gradient layer), and the lower troposphere. The upper troposphere is generally fresh water, which mainly plays the role of maintaining the salinity gradient of the brine in the solar pond and resisting wind disturbances; the middle layer is called the non-troposphere, which has a salinity gradient and temperature gradient from top to bottom, and is the insulation layer of the solar pond; the bottom layer is called the lower troposphere, which is composed of a high-concentration salt solution. Its main function is to collect and store heat, and is used to collect and store solar energy. When solar radiation reaches the surface of the water body, part of it is absorbed, part of it is reflected, and part of it is refracted into the water body. The solar radiation refracted into the water body is absorbed by the water layer by layer, and the remaining part reaches the bottom of the pool and is absorbed by the bottom of the pool, causing the bottom of the pool to heat up. Under normal circumstances, as the temperature of the lower water body increases, thermal convection will naturally form, making the temperature of the entire pool water tend to be balanced. In the solar pool, the salinity gradient will prevent the occurrence of thermal convection. In other words, the density difference formed by the salinity gradient in the solar pool is sufficient to suppress the density difference caused by the temperature gradient, so thermal convection cannot be formed, causing the temperature of the lower troposphere water to gradually rise, forming a temperature gradient from top to bottom and maintaining its thermal stability. In this case, the heat in the lower troposphere can only be transferred upward to the pool surface by heat conduction, while the non-troposphere water layer is very thick, generally up to 1 to 1.5 meters deep, with good thermal insulation properties, and water has a very high thermal resistance (the thermal conductivity of water is 0.654W / m at 60°C). 2·℃), the insulation effect of a 1-meter-thick water layer is equivalent to that of more than ten centimeters of asbestos. Therefore, a "closed system" is formed in the troposphere below the solar pool. Solar radiation continuously enters the bottom of the pool, and the heat energy cannot be dissipated. As a result, the water temperature in the lower troposphere continues to rise and maintains a high temperature, thus forming a high temperature at the bottom of the solar pool, causing the lithium carbonate in the brine to precipitate.

[0004] The salt gradient solar pond process is simple to operate. The production process uses solar energy as the energy source for the evaporation and crystallization process, and uses solar pond technology to obtain lithium carbonate products, which greatly improves the utilization rate of solar energy and makes production safe, harmless and low-cost. The raw brine is used in a closed-loop cycle, and there is no problem of tail brine discharge, so resources are fully utilized. The salt minerals precipitated from the salt field are all soluble substances, which can be dissolved in fresh water and directly returned to the salt lake, without affecting the composition of other components of the salt lake and its future comprehensive development. No chemical reagents are added in each link of the entire process to achieve clean production, and directly obtain a concentrate with a lithium carbonate grade of more than 75%, which is environmentally friendly and a completely green production process.

[0005] However, the traditional salt gradient solar pond technology for lithium extraction requires the occupation of a large area of ​​land to build multi-stage pre-solarization ponds for lithium ion enrichment. In the fragile ecological environment system of Tibet, it is difficult to increase lithium production capacity by adding salt pans. The overall process cycle of lithium ion enrichment in pre-solarization ponds is long, and there is no control standard for ion concentration in brine. It is greatly affected by precipitation and climate, and there is still a situation of "relying on the weather for food". Innovative technologies are needed to scientifically intervene in lithium ion enrichment and reduce the impact of natural conditions such as climate and environment on production. Therefore, researchers are committed to finding a lithium extraction technology that reduces the use of salt pans, scientifically controls brine irrigation, and can adapt to the fragile ecological environment of the plateau. Summary of the invention

[0006] The present invention aims at the problems of large floor space, long cycle and unstable lithium ion enrichment effect in the traditional salt gradient solar pond technology, and provides a method for efficiently extracting lithium from carbonate salt lakes by adsorption coupling salt gradient solar ponds. The raw brine of carbonate salt lakes is pre-adsorbed and desorbed by lithium ion adsorbent, and the lithium ions are enriched and then concentrated by evaporation before brine filling. Compared with the brine obtained by traditional multi-stage brine drying, the lithium ion concentration in the brine of the present invention is increased by more than 9 times, the lithium carbonate precipitation amount is increased by 22.73% compared with the traditional salt gradient solar pond process, and the lithium carbonate crystallization rate is increased by 50%, which greatly improves the efficiency and output of lithium extraction in traditional salt gradient solar ponds.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for extracting lithium from a carbonate salt lake by an adsorption-coupled salt gradient solar pond, comprising the following steps:

[0008] (1) a lithium ion adsorbent is packed into a column to form an adsorption column, carbonate salt lake raw material brine is introduced into the adsorption column until the lithium ion adsorbent is saturated with adsorption, dilute hydrochloric acid is introduced into the adsorption column for column elution, and a desorption liquid rich in lithium ions is collected;

[0009] (2) subjecting the lithium ion-rich desorption solution obtained in step (1) to evaporation and concentration to obtain a lithium solution with a higher lithium ion concentration;

[0010] (3) The lithium solution with a higher lithium ion concentration obtained in step (2) is used as brine and introduced into the lower troposphere of the solar pond to crystallize lithium carbonate, and the lithium carbonate is collected.

[0011] The present invention couples adsorption with salt gradient solar pond technology. No chemical reagents are added in any link of the entire process, and the direct enrichment of lithium ions from carbonate salt lake raw brine is achieved. There is no need to build salt fields or rely on the weather, thus achieving clean production.

[0012] As a preferred embodiment of the method of the present invention, in step (1), the preparation method of the lithium ion adsorbent comprises the following steps:

[0013] S1: calcining a mixture of titanium dioxide and lithium carbonate, eluting lithium ions from the calcined product with a sodium sulfate solution, and then washing, drying and grinding to obtain H2TiO3 nanopowder;

[0014] S2: H2TiO3 nanopowder and polyacrylonitrile fiber are mixed and dispersed in N,N-dimethylformamide, and stirred to form a spinning solution with a mass concentration of 12.5-15wt%, and then electrospun to prepare a lithium ion adsorbent.

[0015] As a preferred embodiment of the method of the present invention, in step S1, the molar ratio of titanium dioxide to lithium carbonate is 1:(1-1.2); the calcination temperature is 800-1100° C., the calcination time is 4.5-6 h; and the concentration of the sodium persulfate solution is 0.4-0.8 mol / L.

[0016] As a preferred embodiment of the method of the present invention, in step S2, the mass ratio of H2TiO3 nanopowder to polyacrylonitrile fiber is (1.4-2):1; the stirring temperature is 80-85°C, and the stirring time is 8-10 hours.

[0017] Experiments have shown that the lithium ion adsorbent prepared within the above parameter range exhibits a better adsorption, desorption and concentration effect on lithium ions in carbonate salt lake brine.

[0018] The lithium ion adsorbent prepared by the present invention is PAN@H2TiO3 nanofiber, the diameter of the fiber does not exceed 300nm, and it shows a more excellent adsorption, desorption and concentration effect on lithium ions in carbonate salt lake brine.

[0019] The lithium ion adsorbent provided by the present invention has a simple preparation process. The prepared lithium ion adsorbent has an adsorption capacity of 16.5 to 18.8 mg / g for lithium ions in carbonate salt lake raw material brine. The lithium ion concentration after adsorption and concentration by the lithium ion adsorbent of the present invention can be increased by 1.97 to 3 times.

[0020] As a preferred embodiment of the method of the present invention, in the step (1), the molar concentration of the dilute hydrochloric acid is 0.4-0.8M, the content of lithium ions in the carbonate salt lake raw brine is 0.45-0.76g / L, and the content of lithium ions in the lithium ion-rich desorption solution is 1.4-2.5g / L.

[0021] As a preferred embodiment of the method of the present invention, in the step (2), the concentration of lithium ions in the lithium solution with a higher lithium ion concentration is 3 to 7 g / L.

[0022] As a preferred embodiment of the method of the present invention, in the step (3), the crystallization saturation time of lithium carbonate in the solar pond is 20 hours, and the grade of the obtained lithium carbonate is greater than 87%.

[0023] As a preferred embodiment of the method of the present invention, in the step (1), before the carbonate salt lake raw brine is introduced into the adsorption column, an activation process of the lithium ion adsorbent is also included, and the specific method is: 0.4-0.8M dilute hydrochloric acid is introduced into the adsorption column at a flow rate of 100-120mL / h to clean and activate the lithium ion adsorbent, and when Li + When the concentration is less than 20 mg / L, the activation of the lithium ion adsorbent is complete.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses fiber-based adsorption materials to enrich and concentrate lithium ions in carbonate salt lake raw material brine. Compared with the lithium ion concentration in the traditional multi-stage brine injection, the lithium ion concentration in the brine after adsorption and concentration is increased by 1.97 to 3 times, and further increased to about 9 times after evaporation and concentration, which greatly increases the concentration of lithium ions in the solution. At the same time, the associated ions such as K + 、Na + The decrease is obvious, which is conducive to the crystallization of lithium carbonate and improves the grade of lithium carbonate.

[0026] (2) The present invention uses high-concentration lithium ion desorption liquid enriched by fiber-based adsorption materials as brine to be directly injected into the lower troposphere of the salt gradient solar pond, coupling adsorption with salt gradient solar pond technology. No chemical reagents are added in each link of the entire process, and the raw brine is directly enriched with lithium ions. There is no need to build salt fields and no longer rely on the weather, and a lithium carbonate concentrate with a grade of 87% or more is directly obtained, realizing clean production; the raw brine is circulated in a closed loop, and resources are fully utilized; compared with the traditional salt gradient solar pond process, the amount of lithium carbonate precipitation is increased by 22.73%, and the lithium carbonate crystallization rate is increased by 50% (in terms of Li + count).

[0027] (3) The process of the present invention is simple, has low operating costs, is suitable for industrial application in carbonate salt lakes, and is environmentally friendly. It is a completely green process and can be widely promoted in the field of lithium extraction from salt lakes on the Qinghai-Tibet Plateau. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the scanning electron microscope (SEM) image of PAN@H2TiO3 nanofibers in Example 1.

[0029] Figure 2 This is a graph showing the cyclic adsorption performance of PAN@H2TiO3 nanofibers in Example 1 for a carbonate brine.

[0030] Figure 3 This is a schematic diagram of the structure of a small solar pond built in the laboratory in Example 2.

[0031] Figure 4 This is a comparison chart of the lithium carbonate crystallization rate between the adsorption-coupled solar pond process and the traditional solar pond process in Example 2.

[0032] Figure 5 This is the process roadmap for lithium extraction from traditional salt gradient solar ponds.

[0033] Figure 6 The process roadmap for lithium extraction by lithium adsorbent adsorption coupled with salt gradient solar pond. DETAILED DESCRIPTION

[0034] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.

[0035] Those skilled in the art should understand that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. The experimental methods used in the examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.

[0036] Example 1

[0037] This embodiment provides a lithium ion adsorbent PAN@H2TiO3 nanofiber, and the preparation method thereof comprises the following steps:

[0038] (1) Mix isopropyl titanate, anhydrous ethanol and deionized water in a volume ratio of 5:100:1, let stand at room temperature for 8 hours, filter and dry the precipitate to obtain amorphous titanium dioxide. Mix titanium dioxide and lithium carbonate in a molar ratio of 1:1, heat the mixture to 900°C at a heating rate of 5°C / min and calcine for 4.5 hours to obtain a product, elute lithium ions with 0.6 mol / L sodium persulfate to obtain H2TiO3, wash the H2TiO3 with ethanol, dry and grind it to obtain H2TiO3 nanopowder.

[0039] (2) H2TiO3 nanopowder and polyacrylonitrile fiber (PAN fiber) were added to N,N-dimethylformamide at a mass ratio of 7:5, and stirred at 85°C for 10 hours to prepare a uniform and transparent spinning solution with a concentration of 13wt%. The spinning was carried out under the conditions of voltage of 15kV and spinning solution flow rate of 0.25mL / min. The product was allowed to stand at room temperature for 48 hours to obtain PAN@H2TiO3 nanofibers, whose electron microscope photos are shown in the figure. Figure 1 As shown, the diameter of PAN@H2TiO3 nanofibers does not exceed 300 nm.

[0040] The raw brine in the Zabuye lithium carbonate salt lake was used as the experimental object to analyze the lithium ion enrichment effect of the lithium ion adsorbent PAN@H2TiO3 nanofiber prepared in this embodiment on the raw brine. The experimental method is as follows:

[0041] Take 1g of PAN@H2TiO3 nanofibers and load them on a glass column with an inner diameter of 6mm and a height of 100mm to carry out a fixed bed adsorption experiment. The experiment was carried out at room temperature. The raw brine shown in Table 1 was pumped into the column from the top of the column at a steady flow rate of 0.5mL / min using a peristaltic pump. After the adsorbent PAN@H2TiO3 nanofibers in the column were saturated with adsorption, 0.5M dilute hydrochloric acid was passed from the top of the column into the column at a flow rate of 1mL / min to elute through the column. The desorbed liquid was collected and the dynamic desorption data of the desorbed liquid was tested. Then, the adsorption column was cleaned with 0.5M dilute hydrochloric acid until Li + The concentration is less than 20 mg / L, and the activation of the adsorbent is considered complete. The raw brine is then adsorbed, desorbed, eluted and the desorbed liquid is collected by a peristaltic pump according to the above method, which represents one cycle. The above adsorption column cleaning activation, raw brine adsorption, desorption, elution and desorption liquid collection are repeated for circulation. The changes in ion types and ion ratios in the desorbed liquid with cycle time are shown in Table 2. The Na + / Li + From 172.67 in the raw brine to 6.15, K+ / Li + From 57.05 in the raw brine to 3.64, comparing the data in Table 1 and Table 2, the concentration of associated ions in the solution was greatly reduced, and Li + The concentration reaches 1.5g / L, which is 1.97 times higher than that of the raw brine, and is more conducive to the crystallization of lithium carbonate in the desorption solution.

[0042] Table 1 Raw brine composition

[0043]

[0044] Table 2 Dynamic desorption data of brine after adsorption and elution by adsorbent

[0045]

[0046] The lithium ion adsorption capacity of lithium ion adsorbent PAN@H2TiO3 nanofiber in carbonate salt lake brine is tested by the following method:

[0047] In a constant temperature oscillator, 0.5 g of adsorbent was added to a capped conical flask containing 50.0 mL of brine, and allowed to stand for adsorption for 5 h. Samples were taken to measure the volume of the adsorbed solution. During the desorption process, the adsorbent was placed in a 60°C oven for 8 h to dry. After drying, it was placed in 50 mL of 0.5 M dilute hydrochloric acid solution for 3 h, and samples were taken to measure the lithium ion concentration in the desorbed solution.

[0048] The adsorption capacity of the adsorbent for lithium ions is calculated according to the following formula:

[0049]

[0050] Where q is the adsorption capacity, expressed in milligrams of lithium ions adsorbed per gram, and its unit is mg / g, c i and c f are the initial and final concentrations of metal lithium ions (mg / L), V is the volume of the solution (L), and m is the mass of the adsorbent (g).

[0051] According to the above method and formula, the adsorption capacity is calculated. The adsorption capacity of lithium ions in carbonate salt lake brine by adsorbent PAN@H2TiO3 nanofiber is as follows: Figure 2 As shown, it is 17.8 mg / g. After the adsorbent is cleaned and activated with 0.5 M dilute hydrochloric acid, and then cyclically adsorbed and desorbed 50 times using the above method, the adsorption capacity is relatively constant and maintained at 16.7 mg / g. As the number of cycles is further increased to 300 times, the adsorption capacity is still relatively constant and maintained between 16.5 and 17 mg / g, indicating that the adsorbent prepared in this example has good adsorption stability and is suitable for industrial application.

[0052] Example 2

[0053] This embodiment provides a method for extracting lithium from a carbonate salt lake by coupling the lithium ion adsorbent prepared in Example 1 with a salt gradient solar pond technology, comprising the following steps:

[0054] (1) Lithium ion enrichment in raw brine from Zabuye lithium carbonate salt lake

[0055] Use a measuring cylinder to measure 50 mL of the adsorbent (PAN@H2TiO3 nanofiber) prepared in Example 1 and load it onto the column. Use 0.5 M dilute hydrochloric acid at a flow rate of 120 mL / h for 3 h to wash it. Take the washing liquid and spot sample to measure Li + concentration, when Li + The concentration is less than 20 mg / L, which means that the adsorbent is activated. + Cleaning qualified.

[0056] Subsequently, the carbonate salt lake raw brine was adsorbed and desorbed using the cleaned adsorbent at room temperature (about 20°C). During the adsorption process, the carbonate salt lake raw brine (lithium ion content is 0.45-0.76g / L) was passed through the column at a flow rate of 150mL / h, and a spot sample was taken every 50mL. The column liquid was collected and stirred evenly, and a mixed sample was taken. During the desorption process, 0.5M dilute hydrochloric acid was passed through the column at a flow rate of 200mL / h, and a spot sample was taken every 100mL. The column liquid was collected and stirred evenly, and a mixed sample was taken.

[0057] (2) When Li + When the concentration reaches 1.5 g / L, Li + The concentration increases slowly, and the desorption liquid is evaporated and concentrated using MVR technology to obtain Li + Concentration 3 ~ 7g / L pure high lithium solution (containing sodium, potassium, Na + / Li + About 6.3; K + / Li + about 3.7).

[0058] (3) The concentrated desorption liquid is used as a brine-injection coupled solar pond to extract lithium carbonate

[0059] An adsorption-coupled solar pool extraction experiment of lithium carbonate was carried out in a small experimental solar pool built in the laboratory. The body of the small laboratory solar pool was made of an outer iron layer, a middle insulation layer and an inner waterproof layer. The middle insulation layer of the pool wall was made of extruded polystyrene foam (XPS) insulation material, and the inner waterproof layer was a high-density polyethylene (HDPE) anti-seepage membrane. Six 300w laboratory xenon lamps were used to simulate the solar light source.

[0060] The total depth of the solar pool is 120cm. Figure 3As shown, it consists of three parts: upper troposphere, non-troposphere and lower troposphere, with thicknesses of 30 cm, 60 cm and 30 cm respectively, and the temperature of the lower troposphere is 55°C. + A pure high-lithium solution with a concentration of 3 to 7 g / L was injected as brine into the lower troposphere of the salt gradient solar pond. Samples were taken every 30 minutes after the injection of brine to test the Li content in the lower troposphere solution. + Concentration, such as Figure 4 shown.

[0061] The comparative experiment directly used the brine in Table 1 to evaporate to Li + The concentration is 3g / L (the Li + The concentration is higher than that of Li in brine made from traditional multi-stage pre-solarization ponds. + The concentration is high) and injected into the salt gradient solar pond as brine. Other conditions remain unchanged. Samples are taken every 30 minutes after the injection of brine to test the Li content in the lower troposphere solution. + Concentration, such as Figure 4 shown.

[0062] Figure 4 The results show that both the traditional solar pond technology and the adsorption-coupled salt gradient solar pond technology can achieve clean production, the raw brine is circulated in a closed loop, and resources are fully utilized; however, the lithium carbonate grade that can be directly obtained from the adsorption-coupled salt gradient solar pond of the present invention is greater than 87% of the concentrate, while the lithium carbonate grade obtained from the traditional solar pond is about 75%. It takes 40 hours for the lithium carbonate in the brine to be crystallized and saturated in the traditional solar pond technology, while the coupling new technology only takes about 20 hours. The crystallization rate of lithium carbonate in the coupling new technology is increased by 50%, and the amount of lithium carbonate precipitation is increased by 22.73% (in terms of Li+) when saturated compared to the traditional salt gradient solar pond process. + count).

[0063] Example 3

[0064] This embodiment provides a method for extracting lithium from a carbonate salt lake by coupling the lithium ion adsorbent prepared in Example 1 with the salt gradient solar pond technology, wherein in step (1), the molar concentration of dilute hydrochloric acid is 0.4 M, and the remaining steps are the same as those in Example 2. The effect of extracting lithium carbonate in this embodiment is the same as that in Example 2.

[0065] Example 4

[0066] This embodiment provides a method for extracting lithium from a carbonate salt lake by coupling the lithium ion adsorbent prepared in Example 1 with the salt gradient solar pond technology, wherein in step (1), the molar concentration of dilute hydrochloric acid is 0.8 M, and the remaining steps are the same as those in Example 2. The effect of extracting lithium carbonate in this embodiment is the same as that in Example 2.

[0067] Although in the same +Under the conditions of concentration, lithium carbonate is prepared by injecting brine into the troposphere below the salt gradient solar pond. However, it can be seen that the grade of lithium carbonate after adsorption coupling is higher, the time for lithium carbonate crystallization adsorption saturation is greatly shortened, and the amount of lithium carbonate precipitation is also significantly increased. This is due to the following reasons:

[0068] First, after selective adsorption by the adsorbent (PAN@H2TiO3 nanofiber) of the present invention, the associated ions are reduced, that is, the sodium ions and potassium ions in the solution are reduced, the associated salts in the lithium carbonate crystallization process are reduced, and the grade of lithium carbonate is improved.

[0069] Secondly, after selective adsorption by the adsorbent (PAN@H2TiO3 nanofibers), the associated cations are reduced, the lithium ion concentration is increased, the binding energy of lithium and carbonate is reduced by the competition between sodium ions, potassium ions, etc. and carbonate, and the crystallization efficiency of lithium carbonate is improved.

[0070] In addition, after selective adsorption by the adsorbent, the lithium ion concentration increases, the supersaturation of lithium carbonate in the solution decreases, and lithium carbonate is more likely to nucleate and crystallize. After the lithium ion concentration increases, the common ion effect increases the amount of lithium carbonate crystals.

[0071] The process of extracting lithium from carbonate salt lakes by using lithium ion adsorbent coupled with salt gradient solar pond technology provided in this embodiment can be scaled up for practical application. The process flow diagram in practical application is shown in FIG. Figure 6 As shown, compared with the traditional multi-stage pre-salt gradient solar pond process for extracting lithium from carbonate salt lakes (such as Figure 5 Compared with the above, the high-concentration lithium ion desorption liquid of the raw brine after enrichment by fiber-based adsorption materials is directly injected into the lower troposphere of the salt gradient solar pond as brine. No chemical reagents are added in each link of the whole process, which realizes the direct enrichment of lithium ions in the raw brine. There is no need to build salt fields and no longer rely on the weather. The concentrate with a lithium carbonate grade of 87% or more can be directly obtained, realizing clean production.

[0072] Compared with the traditional salt gradient solar pond process, the amount of lithium carbonate precipitation is increased by 22.73%, and the crystallization rate of lithium carbonate is increased by 50% (in terms of Li + The process of the present invention is simple, the operation cost is low, it is suitable for industrial application in carbonate salt lakes, and it is environmentally friendly. It is a completely green process and can be widely promoted in the field of lithium extraction from salt lakes on the Qinghai-Tibet Plateau.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for extracting lithium from carbonate salt lakes by adsorption-coupled salt gradient solar ponds. It is characterized in that The steps are: (1) a lithium ion adsorbent is packed into a column to form an adsorption column, carbonate salt lake raw material brine is introduced into the adsorption column until the lithium ion adsorbent is saturated with adsorption, dilute hydrochloric acid is introduced into the adsorption column for column elution, and a desorption liquid rich in lithium ions is collected; (2) subjecting the lithium ion-rich desorption solution obtained in step (1) to evaporation and concentration to obtain a lithium solution with a higher lithium ion concentration; (3) using the lithium solution with a higher lithium ion concentration obtained in step (2) as irrigation brine, passing it into the lower troposphere of the solar pond to crystallize lithium carbonate, and collecting the lithium carbonate; In the step (2), the concentration of lithium ions in the lithium solution with a higher lithium ion concentration is 3 to 7 g / L; In the step (3), the temperature of the troposphere below the solar pond is 55°C.

2. The method according to claim 1, It is characterized in that In the step (1), the preparation method of the lithium ion adsorbent comprises the following steps: S1: The mixture of titanium dioxide and lithium carbonate is roasted, and the roasted product is washed with sodium sulfate solution to remove lithium ions, and then washed, dried and ground to obtain H 2 TiO 3 Nano powder; S2: H 2 TiO 3 The nano powder and polyacrylonitrile fiber are mixed and dispersed in N,N-dimethylformamide, and a spinning solution with a mass concentration of 12.5-15wt% is formed by stirring, and then a lithium ion adsorbent is prepared by electrostatic spinning.

3. The method according to claim 2, It is characterized in that In the step S1, the molar ratio of titanium dioxide to lithium carbonate is 1:(1-1.2); the roasting temperature is 800-1100° C., the roasting time is 4.5-6 hours; and the concentration of the sodium persulfate solution is 0.4-0.8 mol / L.

4. The method according to claim 2, It is characterized in that In step S2, H 2 TiO 3 The mass ratio of nano powder to polyacrylonitrile fiber is (1.4-2):1; the stirring temperature is 80-85°C, and the stirring time is 8-10h.

5. The method according to claim 2, It is characterized in that In the step S2, the diameter of the fibers in the lithium ion adsorbent does not exceed 300 nm.

6. The method according to claim 2, It is characterized in that In the step S2, the adsorption capacity of the lithium ion adsorbent for lithium ions in the carbonate salt lake raw material brine is 16.5-18.8 mg / g.

7. The method according to claim 1, It is characterized in that In the step (1), the molar concentration of the dilute hydrochloric acid is 0.4-0.8 M, the content of lithium ions in the carbonate salt lake raw brine is 0.45-0.76 g / L, and the content of lithium ions in the lithium ion-rich desorption solution is 1.4-2.5 g / L.

8. The method according to claim 1, It is characterized in that In the step (3), the crystallization saturation time of lithium carbonate in the solar pond is 20 hours.

9. The method according to claim 1, It is characterized in that In the step (1), before the carbonate salt lake raw material brine is introduced into the adsorption column, the activation process of the lithium ion adsorbent is also included, and the specific method is: 0.4-0.8M dilute hydrochloric acid is introduced into the adsorption column at a flow rate of 100-120mL / h to clean and activate the lithium ion adsorbent; when Li + When the concentration is less than 20 mg / L, the activation of the lithium ion adsorbent is complete.

Citation Information

Patent Citations

  • Method for preparing lithium carbonate from salt lake brine

    CN111792657A

  • Preparation method of porous spinning composite material and lithium extraction application thereof

    CN112619621A

  • Method for extracting lithium from carbonate brine

    CN115321561A

  • Crown ether carrier-containing nanofiber material for adsorbing lithium ions and preparation method of crown ether carrier-containing nanofiber material

    CN115369510A

  • Lithium ion adsorption material, preparation method thereof, lithium extraction system and lithium extraction method

    CN115970659A