A chemical tin precipitation composite solution, tin precipitation process and application thereof

Through the chemical immersion tin compound solution and specific process steps, a stable and uniform tin layer is formed, which solves the problem of the metal protective layer being volatile and uneven at high temperatures, meets the high temperature stability and density requirements of the printed circuit board, and achieves The excellent performance and cost reduction of the tin layer are achieved.

CN117888094BActive Publication Date: 2024-10-29中山博美新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311787380.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-10-29
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

The preparation process of the metal protective layer in the prior art is difficult to meet the stability and uniformity requirements of printed circuit board circuit densification and high-temperature environments, resulting in the tin layer being prone to volatilization and unevenness at high temperatures.

Method used

Using a chemical tin immersion composite solution, including tin base agent, tin correction agent, SnTech tin solution and special acid, a silvery white dense tin layer is formed through a displacement reaction, combined with specific process steps such as pre-immersion and post-immersion. Tin treatment, control tin layer thickness and stability.

Benefits of technology

It achieves high stability and uniformity of the tin layer. The thickness of the tin layer can be controlled at more than 1 micron, which meets the multiple welding requirements of the lead-free assembly process. The flatness and thickness distribution uniformity of the tin surface are excellent, and the length and number of tin whiskers meet the requirements. Strict standards reduce costs and customer wastewater treatment pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004625476320000091
    Figure BDA0004625476320000091
  • Figure HDA0004625476540000011
    Figure HDA0004625476540000011
  • Figure HDA0004625476540000012
    Figure HDA0004625476540000012
Patent Text Reader

Abstract

The present invention relates to the field of printed circuit board surface treatment, and discloses a chemical tinning composite solution, a tinning process and applications thereof. The chemical tinning composite solution of the present invention comprises a tinning base agent, a tinning corrector, a SnTech tin solution, a special acid SF and a tinning additive. The chemical tinning process of the present invention comprises acid degreasing, microetching, pre-immersion, chemical tinning, post-tinning, water washing and anti-oxidation washing of a board to be treated in sequence, wherein the pre-immersion, chemical tinning and post-tinning adopt the chemical tinning composite solution of the present invention, which has excellent tinning performance and tin whisker suppression ability, and the obtained tinning layer has the longest tin whisker length and quantity that can meet the most stringent IPC‑4554 standard during storage, and has a wide range of application value in the field of chemical tinning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of printed circuit board surface treatment, in particular to a chemical tin precipitation composite solution, a tin precipitation process and applications thereof. Background Art

[0002] Printed circuit board (PCB) is a printed board with point connections and printed components formed on a general substrate according to a predetermined design. Its main function is to connect various electronic components to form a predetermined circuit, play the role of relay transmission, and is a key electronic interconnection component of electronic products. After the printed circuit board is completed, the exposed copper wire on its surface needs to be protected. Usually, technicians will deposit a layer of protective film on the exposed surface of the copper wire to prevent the exposed copper wire from being oxidized or sulfurized during the component packaging process to avoid affecting the subsequent packaging (such as reflow soldering or gold wire soldering, etc.).

[0003] In the related art, the deposited protective layer can be divided into an organic soldering layer and a metal protective layer according to the difference in properties. The organic soldering layer is formed by coating a layer of organic coating on the surface of the copper wire. It has excellent specificity for copper and will not be adsorbed on the insulating coating. However, the high temperature resistance of the organic soldering layer is poor. Especially in reflow soldering, the organic soldering layer is easy to volatilize due to the high temperature, which causes the film layer to be melted. The metal protective layer is currently the mainstream deposited protective layer. Its preparation process includes hot air leveling, chemical tin precipitation, chemical silver precipitation, etc. Although it can make up for the defects of the organic soldering layer to a certain extent, as electronic products are transformed into lightweight and miniaturized, the circuits of printed circuit boards become more dense, which puts forward higher requirements on the uniformity, stability and film thickness of the metal protective layer. However, the preparation process of the metal protective layer in the related art is difficult to meet the above requirements.

[0004] Therefore, there is an urgent need to seek a chemical tinning process and its application, and the tinning board produced by the process has excellent stability and tinning performance. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a chemical tinning composite solution, which can effectively improve the tinning performance of the product and has excellent tin whisker suppression ability. During the storage process of the tinning layer, the longest tin whisker length and number can fully comply with the most stringent IPC-4554 standard and be controlled within 50 microns.

[0006] The invention also provides a chemical tin deposition process.

[0007] The invention also proposes the application of a chemical tin precipitation composite solution or a chemical tin precipitation process in preparing a tin precipitation layer.

[0008] In a first aspect of the present invention, a chemical tin immersion composite solution is provided, wherein the raw materials for preparing the chemical tin immersion composite solution include a tin immersion base agent, a tin immersion corrector SN, a SnTech tin solution, a special acid SF and a tin immersion additive, wherein:

[0009] The tin-containing basic agent comprises thiourea, citric acid and tartaric acid;

[0010] The tin calibrant comprises sodium hypophosphite;

[0011] The SnTech tin solution includes tin methanesulfonate;

[0012] The special acid SF comprises methanesulfonic acid;

[0013] The tin additive comprises polyether P-65 and PEG.

[0014] The chemical tin immersion composite solution according to the embodiment of the present invention has at least the following beneficial effects:

[0015] (1) The chemical tin immersion composite solution of the present invention does not contain lead and complies with RoHS regulations.

[0016] (2) The chemical tinning composite solution of the present invention is suitable for various PCB boards, with good flatness and uniform thickness distribution, and the prepared tin layer can easily reach more than 1 micron, and the thickness of the tin layer can reach up to 1.5 microns (conventionally controlled 0.8-1.3um), which can meet the multiple welding requirements of the lead-free assembly process (2 reflow soldering + 1 wave soldering);

[0017] (3) The chemical tin precipitation composite solution of the present invention is used for tin precipitation treatment. Through the replacement reaction, a tin layer of about 1 micron, silvery white matte, dense, and free of tin whiskers or dendritic crystals can be deposited on the copper surface. The tin layer has good tin surface flatness and excellent tin thickness distribution uniformity (Cpk>1.33).

[0018] In some embodiments of the present invention, the concentration of the tin base agent in the chemical tin precipitation composite solution is 700-730 ml / L, the concentration of the tin correction agent SN is 140-170 ml / L, the concentration of the SnTech tin solution is 50-60 ml / L, the concentration of the special acid SF is 50-70 ml / L, and the concentration of the tin additive is 0.5-1 ml / L.

[0019] In some embodiments of the present invention, the concentration of thiourea in the tin-containing basic agent is 120-140 g / L, the concentration of citric acid is 20-40 g / L, and the concentration of tartaric acid is 20-40 g / L;

[0020] The concentration of the sodium hypophosphite in the tin oxide calibration agent is 20-40 g / L;

[0021] The concentration of tin methanesulfonate in the SnTech tin solution is 290-310 g / L

[0022] The concentration of methanesulfonic acid in the special acid SF is 670-730 g / L;

[0023] The concentration of the polyether P-65 in the tin additive is 5-20 g / L, and the concentration of the PEG is 10-30 ml / L.

[0024] In some embodiments of the present invention, the PEG is PEG1450.

[0025] A second aspect of the present invention provides a chemical tinning process, which specifically comprises the following steps:

[0026] Step S1, soaking the board to be treated in a solution containing an acidic degreasing agent, washing with water, and obtaining a degreasing board;

[0027] Step S2, placing the degreased plate in a micro-etching salt solution for treatment, and washing with water to obtain a micro-etching plate;

[0028] Step S3, placing the micro-etched board in the chemical tin immersion composite solution of the first aspect for pre-preg treatment to obtain a pre-preg board;

[0029] Step S4, continuing to immerse the pre-impregnated board in the chemical tin immersion composite solution for chemical tin immersion treatment to obtain a chemical tin immersion board, and then placing the chemical tin immersion board in the chemical tin immersion composite solution with a concentration of 40 to 60% (V / V) for post-tin immersion treatment;

[0030] Step S5, washing the chemical tin-immersion plate after the post-tinning treatment with water and / or anti-oxidation washing in sequence, and then drying it.

[0031] The preparation process according to the embodiment of the present invention has at least the following beneficial effects:

[0032] (1) The chemical tinning process of the present invention is applicable to both horizontal tinning lines and vertical tinning lines, and has good process control stability and simple operation.

[0033] (2) The chemical tinning process of the present invention can accurately control the thickness of the tin layer by controlling the chemical tinning time, and the tin surface of the obtained tinning layer does not turn yellow after three reflows during lead-free soldering in an air environment.

[0034] (3) During the post-tinning process, by adjusting the chemical tinning composite solution to 40-60%, not only can the difficulty of board cleaning be reduced, but also the amount of chemical solution carried out can be reduced, thereby reducing costs and customer wastewater treatment pressure.

[0035] In some embodiments of the present invention, in step S1, the volume fraction of the acidic degreasing agent is 18% to 25%, preferably 19% to 23%.

[0036] In some embodiments of the present invention, in step S1, the soaking temperature is 35 to 50°C;

[0037] Preferably, the soaking time is 45 to 90 seconds.

[0038] In some embodiments of the present invention, in step S2, the concentration of the micro-etching salt is 35-45 g / L.

[0039] In some embodiments of the present invention, in step S2, the treatment temperature is 25-40° C.; preferably, the treatment time is 45-120 s.

[0040] In some embodiments of the present invention, in step S3, the prepreg treatment temperature is 20 to 30°C;

[0041] Preferably, the prepreg treatment time is 45 to 90 seconds.

[0042] In some embodiments of the present invention, in step S4, the temperature of the chemical tin treatment is 68-73° C., and the time of the chemical tin treatment is 12-21 min.

[0043] In some embodiments of the present invention, the concentration of the chemical tin composite solution of the post-tin treatment is 40-60% (V / V).

[0044] In some embodiments of the present invention, the temperature of the post-tinning treatment is 50-70° C., and the treatment time is 20-90 seconds.

[0045] In some embodiments of the present invention, in step S4, the water washing includes single-stage water washing or thiourea washing and deionized water washing.

[0046] In some embodiments of the present invention, when the chemical tinning process is a vertical tinning process, in step S4, the water washing includes thiourea washing and deionized washing.

[0047] Thiourea can complex with free copper ions to form a copper-thiourea complex, preventing the free copper ions from reversely depositing on the tin surface, thereby affecting the quality of the tin surface.

[0048] In some embodiments of the present invention, the thiourea washing is washing with thiourea or AR grade sulfuric acid solution.

[0049] In some embodiments of the present invention, when the chemical immersion tin process is a horizontal immersion tin process, in step S4, the water washing includes single-stage water washing and deionized washing.

[0050] In some embodiments of the present invention, the deionized water solution contains an alkaline detergent, and the concentration of the alkaline detergent is 2-5% (v / v).

[0051] In some embodiments of the present invention, the concentration of the alkaline cleaning agent is 4% (v / v).

[0052] In some embodiments of the present invention, the alkaline cleaning agent is selected from at least one of the deionized cleaning agent 100 or the deionized cleaning agent SF 800.

[0053] Deionized cleaning agent 100 / SF800 is an alkaline cleaning agent that can effectively neutralize the acidic substances remaining on the board surface, reduce the ion residues on the solder mask ink layer and the tin surface, and effectively improve the ion contamination problem.

[0054] In some embodiments of the present invention, the deionized water solution contains NaCl.

[0055] Specifically, the concentration of NaCl in the deionized water solution is less than 0.5 μg / cm 2 , which can effectively reduce ion contamination.

[0056] In some embodiments of the present invention, the anti-oxidation washing solvent includes an anti-oxidation cleaning agent.

[0057] The use of the antioxidant cleaning agent of the present invention for cleaning can ensure that the tin surface does not turn yellow after three reflows during lead-free soldering in an air environment.

[0058] In some embodiments of the present invention, the temperature of the anti-oxidation washing is 20 to 30° C., and preferably, the time of the anti-oxidation washing is 10 to 25 seconds.

[0059] Anti-oxidation washing can form an inorganic protective layer on the tin surface to prevent the tin surface from discoloring during reflow soldering in an air environment. This cleaning method is an optional process. PCB manufacturers can decide whether to use it based on the specific conditions of their customers' reflow ovens (whether there is nitrogen protection). The solution is pre-prepared and then added in an overflow manner.

[0060] The third aspect of the present invention provides an application of a chemical tin precipitation composite solution or a chemical tin precipitation process in preparing a tin precipitation layer.

[0061] According to the application of the embodiment of the present invention, at least the following beneficial effects are achieved: the thickness of the tin layer prepared by the chemical tin precipitation composite solution or chemical tin precipitation process of the present invention is highly controllable, and the thickness of the tin layer is evenly distributed, and the maximum thickness can reach 1.5 microns, and the conventional thickness is controlled to be 0.8 to 1.3 microns; secondly, the tin layer prepared by the present invention has excellent corrosion resistance,

[0062] In some embodiments of the present invention, the tin-immersion layer comprises a tin-immersion layer of a printed circuit board.

[0063] In some embodiments of the present invention, unless otherwise specified, the solvent of the solution is water.

[0064] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0066] Figure 1 This is a front view of the tin-immersion PCB board prepared in Example 1 of the present invention.

[0067] Figure 2 This is a back view of the tin-immersion PCB board prepared in Example 1 of the present invention.

[0068] Figure 3 This is a graph showing the anti-aging results of an immersion tin PCB board prepared by the method of Example 1 of the present invention, wherein A is an untreated group, B is an aging treatment under baking conditions of 155° C. for 4 hours, C is a 1-fold reflow aging treatment, and D is a 2-fold reflow aging treatment.

[0069] Figure 4 This is a SEM image of the surface of the tin layer of the tin-immersion PCB board prepared by the method of Example 1 of the present invention.

[0070] Figure 5 This is an EDX image of the surface of the tin layer of the tin-immersion PCB board prepared by the method of Example 1 of the present invention.

[0071] Figure 6 This is the SEM image of the tin layer surface of the tin-immersion PCB board after 1x reflow aging.

[0072] Figure 7 This is the EDX image of the tin layer surface of the tin-immersion PCB board after 1x reflow aging.

[0073] Figure 8 This is the SEM image of the tin layer surface of the tin-immersion PCB board after 2 times reflow aging.

[0074] Fig. 9 This is the EDX image of the tin layer surface of the tin-immersion PCB board after 3 times reflow aging.

[0075] Fig.10 The thickness variation of the intermetallic compound layer (IMC) of the chemical tinning PCB board after treatment under different conditions.

[0076] Fig.11This is the PCB picture after being processed by chemical tinning PCB board + tin paste printing group.

[0077] Fig.12 The results of solder paste printing test on chemical tinning PCB boards under different conditions.

[0078] Fig.13 Float solder test results for through holes.

[0079] Fig.14 It is an untreated chemical tinned PCB board.

[0080] Fig.15 The figure shows the solder mask adhesion performance test results of chemical tinning PCB board.

[0081] Fig.16 The corrosion resistance test results of the tin-immersion PCB board prepared by the method of Example 1 of the present invention are shown.

[0082] Fig.17 The tin whisker detection result of the immersion tin PCB board prepared by the method of Example 1 of the present invention is shown in FIG. DETAILED DESCRIPTION

[0083] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0084] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0085] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0086] Example 1

[0087] This embodiment provides a chemical tinning composite solution suitable for a horizontal tinning process, and the contents of each component thereof are shown in Table 1.

[0088] Table 1: Chemical tin complex solution

[0089] Components Where to buy Addition amount Tin Basic Agent H Plus Zhongshan Bomei Company's own products 729.25mL / L Special acid SF Zhongshan Bomei Company's own products 60mL / L Tin calibrant SN Zhongshan Bomei Company's own products 155mL / L SnTech Tin Solutions Zhongshan Bomei Company's own products 55mL / L Tin Additive C Zhongshan Bomei Company's own products 0.75mL / L

[0090] Among them, the tin-based agent H PLUS is composed of 130g / L thiourea, 30g / L citric acid, 30g / L tartaric acid and water;

[0091] The special acid SF is a methanesulfonic acid solution with a concentration of 700 g / L;

[0092] SnTech tin solution is a 300g / L tin methanesulfonate solution;

[0093] The tin calibrant SN is a sodium hypophosphite solution with a concentration of 30 g / L;

[0094] Tin additive C is composed of 10 g / L polyether P-65, 20 ml / L PEG1450 (BASF) and water.

[0095] This embodiment also provides a PCB board chemical tinning process based on the above chemical tinning composite solution, which specifically includes the following steps:

[0096] Step S1, acid degreasing: place the PCR plate to be treated in a container filled with an acid degreasing agent with a concentration of 21% (v / v) for treatment at a temperature of 40°C for 1 min. After the treatment, perform three-stage water washing for 30 s.

[0097] Step S2, micro-etching: take out the PCR board after three-stage countercurrent water washing, and then put it into a micro-etching salt solution with a concentration of 40g / L at 30°C for 90s to etch away about 1 micron of the copper layer, and then take out the PCB board for three-stage water washing, and the washing time is 30s.

[0098] Step S3, pre-dip: at 25°C, slowly place the PCR plate treated in step S2 into the above-mentioned tin immersion composite solution for pre-dip treatment for 60 seconds to form a dense transition layer on its surface to ensure the reliability of the blind hole while improving the soldering performance of the tin surface.

[0099] Step S4, chemical tinning: After the pre-immersion is completed, the PCB board is placed in the above-mentioned tinning composite solution with a concentration of 100% (v / v) for chemical tinning treatment. The treatment temperature is 70°C and the treatment time is 16 minutes. During the tinning process, the thickness of the deposition can be controlled by adjusting the treatment time;

[0100] Step S5, post-tinning: placing the PCB board after chemical tinning into the above-mentioned tinning composite solution with a concentration of 50% (v / v) for post-tinning treatment, the treatment temperature is 60° C., and the treatment time is 30 seconds.

[0101] Step S6, water washing: the PCB board treated in step S5 is subjected to single-stage water washing at 25° C. for 20 to 30 seconds. After the water washing is completed, the PCB board is taken out and placed in a deionized detergent 100 with a concentration of 40% (v / v) for deionized water washing. The deionized water washing temperature is 50° C. for 120 seconds.

[0102] Step S7, anti-oxidation washing: at 25°C, the PCB board after water washing in step S6 is placed in a 1% (V / V) anti-oxidation cleaning agent 8C solution for 10 to 25 seconds to obtain a chemical tinning PCB board.

[0103] Example 2

[0104] The difference between this embodiment and the above-mentioned embodiment 1 is that the treatment time of the chemical tin precipitation in step S4 is 12 minutes, and the other conditions remain unchanged.

[0105] Example 3

[0106] The difference between this embodiment and the above-mentioned embodiment 1 is that the treatment time of the chemical tin precipitation in step S4 is 20 minutes, and the other conditions remain unchanged.

[0107] Test example 1: tin layer thickness test

[0108] The thickness of the tin-immersion layer of the above-mentioned embodiment 1, embodiment 2 and embodiment 3 was tested, wherein the tin-immersion PCB board obtained by the method of embodiment 1 is as follows Figure 1 and Figure 2 As shown (chemical tin treatment time is 16 minutes), Figure 1 This is the front side of the tinned PCB board. Figure 2 The back side of the tin-immersed PCB board. Furthermore, 10 points were taken on the front side and the back side of the tin-immersed PCB board respectively to measure the tin thickness using X-rays. The results are shown in Table 2.

[0109] Table 2: X-ray tin thickness measurement results

[0110]

[0111] It can be seen that the tin layer thickness of the tin-immersion PCB board obtained by using the chemical tin-immersion composite solution and the tin-immersion process of the present invention is uniform, and the total thickness of the tin-immersion layer is about 1.255 μm.

[0112] Furthermore, the same method was used to detect the total thickness of the tin-immersion layer of Example 2 and Example 3, and the results showed that the total thickness of the tin-immersion layer prepared by the tin-immersion composite solution and tin-immersion process of Example 2 was approximately 0.951 μm; the total thickness of the tin-immersion layer prepared by the tin-immersion composite solution and tin-immersion process of Example 3 was approximately 1.412 μm.

[0113] In summary, it can be seen that the total thickness of the tin layer of the tin-immersion PCB board obtained by the chemical tin-immersion composite solution and the tin-immersion process of the present invention is uniform, and the thickness of the tin layer can be accurately controlled by controlling the chemical tin-immersion time.

[0114] Test example 2: Pure tin layer performance test

[0115] 1. Thickness test

[0116] The method of Example 1 was used to prepare a chemical tin-immersion PCB board, and then the prepared chemical tin-immersion PCB board was subjected to no reflow, primary reflow and secondary reflow treatments, respectively. The test results are shown in Table 3.

[0117] Table 3: Pure tin layer thickness test

[0118] Test conditions Pure tin layer thickness (μm) Test Results No reflow 0.946 Meets OEM assembly requirements One-time reflow 0.209 Meets OEM assembly requirements Secondary reflow 0.116 Meets OEM assembly requirements

[0119] 2. Anti-aging test

[0120] The aging resistance of the tin layer of the chemical tin PCB board prepared by the method of the above embodiment 1 was tested. The chemical tin PCB board prepared by the method of the above embodiment 1 was placed under baking conditions of 155° C. for aging for 4 hours, and then subjected to 1 times reflow aging treatment and 2 times reflow aging treatment.

[0121] The results are as follows Figure 3 As shown, A is the untreated group, B is the aging treatment under baking conditions of 155°C for 4 hours, C is the 1-fold reflow aging treatment, and D is the 2-fold reflow aging treatment. It is shown that under all test conditions, no discoloration was found on the tin surface, and the tin layer of the tin-immersion PCB board obtained by using the chemical tin-immersion composite solution and the tin-immersion process of the present invention has excellent stability.

[0122] 3. Scanning electron microscopy and energy spectrum analysis

[0123] In order to intuitively demonstrate the chemical immersion tin PCB board prepared by the present invention, this experiment carried out scanning electron microscopic observation and energy spectrum analysis on the chemical immersion tin PCB board prepared in Example 1 under different treatment conditions, wherein the conditions were set as follows:

[0124] A: Untreated;

[0125] B: 1x post-reflow aging treatment;

[0126] C: 2 times post-reflow aging treatment.

[0127] Test results such as Figures 4 to 9 As shown, Figure 4 This is a scanning electron micrograph of the tin surface of an untreated chemical tinning PCB board. Figure 5 This is the tin surface energy spectrum analysis diagram of the untreated chemical tin PCB board; Figure 6 This is a scanning electron micrograph of the tin surface of a chemical tin-immersion PCB board after 1x reflow aging treatment. Figure 7 This is the tin surface energy spectrum analysis diagram of the chemical tin PCB board after 1x reflow aging treatment; Figure 8 This is a scanning electron micrograph of the tin surface of a chemical immersion tin PCB board after 2x reflow aging treatment. Fig. 9 This is the tin surface spectrum analysis diagram of the chemical tin PCB board after 2 times reflow aging treatment. The scanning electron microscope analysis results show that the tin crystal structure is normal, and the EDX results show that the tin surface is very clean and there is no pollution on the tin surface.

[0128] Test example 3: Intermetallic compound layer thickness test

[0129] A chemical tinning PCB board was prepared by the method of the above-mentioned embodiment 1 (wherein the chemical tinning treatment time was 15 min), and then placed under different conditions for treatment, and then the thickness change of the intermetallic compound layer (IMC) was detected, wherein the conditions were set as follows:

[0130] ①Store at room temperature for 21 months;

[0131] ② Treat at 155℃ for 2 hours;

[0132] ③ Treat at 155℃ for 4 hours;

[0133] ④One-time reflux treatment;

[0134] ⑤One reflow aging treatment;

[0135] ⑥ Secondary reflux treatment.

[0136] The IMC calculation formula is as follows:

[0137] IMC thickness = total tin layer thickness - pure tin layer thickness,

[0138] The thickness of the total tin layer is measured by the XRF method, and the thickness of the pure tin layer is measured by the SERA method.

[0139] The test results are as follows Fig.10 As shown, the results show that the average IMC thickness of the chemical tin PCB board prepared by the present invention is 0.31 microns after being stored at room temperature for 21 months. The chemical tin PCB board prepared by the present invention was treated at 155°C for 2 hours and 4 hours respectively, and the test results showed that the average IMC thickness was 0.45 microns and 0.56 microns; the chemical tin PCB board prepared by the present invention was subjected to two reflow treatments at 240°C, and the results showed that the intermetallic compound layer could still be controlled within 1 micron, and the pure tin layer had no obvious change.

[0140] Test Example 4: Solderability and Adhesion Test

[0141] 1. Solder paste printing test

[0142] The tinning performance of the chemical immersion tin PCB boards prepared in the above Example 1 was tested and divided into Group A, Group B, Group C and Group D respectively.

[0143] Group A is a chemical tinning PCB board + printing solder paste group, Group B is a chemical tinning PCB board + printing flux paste + reflow oven group, Group C is a chemical tinning PCB board + 1 reflow oven + printing solder paste + reflow oven group, and Group D is a chemical tinning PCB board + 2 reflow ovens + printing solder paste + reflow oven group. In this test example, the type of solder paste is Senju M705-GRN360-K2-V, and the alloy is Sn96.5 / Ag3.0 / Cu0.5.

[0144] Test results such as Fig.11 and Fig.12 As shown, Fig.11 This is the PCB picture after group A solder paste printing. Fig.12 These are the test results for Group B, Group C and Group D. From the test results, it can be seen that Group A, Group B, Group C and Group D have no tin shrinkage phenomenon and the tinning is normal.

[0145] 2. Float solder test for through holes

[0146] This experiment tests the effect of reflow treatment on the through-holes of the chemical tin-immersion PCB board prepared in the above-mentioned embodiment 1, wherein the solder used is lead-free solder and the treatment time is 5s.

[0147] Test results such as Fig.13 As shown, group A was untreated; group B was treated with 1-fold reflow aging; group C was treated with 2-fold reflow aging, showing no effect before and after treatment.

[0148] 3. Adhesion performance test

[0149] The solder mask adhesion performance of the chemical tin PCB board prepared in Example 1 was tested by 3M tape method. The test results are as follows: Fig.14 and Fig.15 As shown, Fig.14 For untreated chemical tin PCB board, Fig.15 The results of the tape test show that no obvious solder mask or tin layer peeling problem was found, indicating that the tin layer of the tin-immersion PCB board obtained by using the chemical tin-immersion composite solution and tin-immersion process of the present invention has excellent anti-adhesion performance.

[0150] Test Example 5: Corrosion Resistance Test

[0151] The chemical tin immersion PCB board prepared in the above embodiment 1 was subjected to sulfur dioxide test, Kjeldahl corrosion test, salt spray test and surface insulation resistance test to detect its corrosion resistance.

[0152] The test results are as follows Fig.16 As shown, it can be seen from the test results that the chemical immersion tin PCB board prepared by the present invention can show excellent corrosion resistance in several conventional corrosion resistance tests.

[0153] Test Example 6: Tin Whisker Suppression Test

[0154] Tin whisker observation was performed on the chemical tin-immersion PCB board prepared in Example 1, and 4 detection points were randomly selected. The detection results are as follows: Fig.17 As shown, it is shown that the chemical immersion tin PCB board prepared by using the chemical immersion tin composite solution of the present invention has excellent tin whisker suppression ability.

[0155] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A chemical tin immersion composite solution, characterized in that: The raw materials for preparing the chemical tin immersion composite solution include: 700-730 ml / L tin base agent, 140-170 ml / L tin correction agent, 50-60 ml / L SnTech tin solution, 50-70 ml / L special acid SF and 0.5-1 ml / L tin additive, wherein: The tin-containing basic agent is composed of 120-140 g / L thiourea, 20-40 g / L citric acid, 20-40 g / L tartaric acid and water; The tin oxide calibration agent is 20-40 g / L sodium hypophosphite solution; The SnTech tin solution is a 290-310 g / L tin methanesulfonate solution; The special acid SF is 670-730 g / L methanesulfonic acid solution; The tin additive consists of 5-20 g / L polyether P-65, 10-30 ml / L PEG and water.

2. The chemical tin immersion composite solution according to claim 1, characterized in that: The PEG is PEG1450.

3. A chemical tinning process, characterized in that: The following steps are involved: Step S1, soaking the board to be treated in a solution containing an acidic degreasing agent, washing with water, and obtaining a degreasing board; Step S2, placing the degreased plate in a micro-etching salt solution for treatment, and washing with water to obtain a micro-etching plate; Step S3, placing the micro-etched board in the chemical tin immersion composite solution of claim 1 or 2 for pre-preg treatment to obtain a pre-preg board; Step S4, continuing to immerse the pre-impregnated board in the chemical tin immersion composite solution for chemical tin immersion treatment to obtain a chemical tin immersion board, and then placing the chemical tin immersion board in the chemical tin immersion composite solution with a concentration of 40-60% (V / V) for post-tin immersion treatment; Step S5, washing the chemical tin-immersion plate after the post-tinning treatment with water and / or anti-oxidation washing in sequence, and then drying it.

4. The chemical tinning process according to claim 3, characterized in that: In step S1, the soaking temperature is 35-50° C., and / or the soaking time is 45-90 seconds.

5. The chemical tinning process according to claim 3, characterized in that: In step S2, the treatment temperature is 25-40°C; and / or the treatment time is 45-120s.

6. The chemical tinning process according to claim 3, characterized in that: In step S3, the prepreg treatment temperature is 20-30° C.; and / or the prepreg treatment time is 45-90 seconds.

7. The chemical tinning process according to claim 3, characterized in that: In step S4, the temperature of the chemical tin treatment is 68-73° C., and / or the time of the chemical tin treatment is 12-21 min.

8. The chemical tinning process according to claim 3, characterized in that: The temperature of the post-tinning treatment is 50-70° C., and / or the time of the post-tinning treatment is 20-90 seconds.

9. Use of the chemical tin precipitation composite solution as claimed in claim 1 or 2 or the chemical tin precipitation process as claimed in any one of claims 3 to 8 in preparing a tin precipitation layer.