Preparation method and application of nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material
By preparing nitrogen-doped iron-cobalt selenide/carbon nanotube composite electrode materials, the problems of limited active sites and unsatisfactory conductivity of existing selenides in the electrochemical field have been solved, and highly sensitive detection of nonsteroidal anti-inflammatory drugs has been achieved.
Patent Information
- Application Number
- CN202410148393.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-02-01
AI Technical Summary
When selenides are used alone in the field of electrochemistry, their active sites are limited and their conductivity is not ideal, making it difficult to construct highly sensitive electrochemical sensors to detect nonsteroidal anti-inflammatory drugs.
An electrochemical sensor was constructed using a nitrogen-doped iron-cobalt-selenide/carbon nanotube composite electrode material. This sensor was developed through morphology control and electronegative heteroatom doping to achieve sensitive detection of the nonsteroidal anti-inflammatory drug ibuprofen.
The prepared composite electrode material has abundant porosity, good conductivity and multiple electroactive sites, which enhances the electrochemical oxidation ability of ibuprofen and achieves highly sensitive detection of ibuprofen.
Smart Images

Figure CN117912856B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method of a composite electrode material and application thereof. Background Art
[0002] Considering that drugs belong to the emerging class of pollutants, the presence of drugs in the environment has received increasing attention. Nonsteroidal anti-inflammatory drugs are a global best-selling over-the-counter drug. Due to their effective antipyretic, analgesic and anti-inflammatory properties, they have become the first choice for various short-term nonspecific pain indications. Especially during the Covid-19 pandemic, they have been widely used in front-line clinics and have been characterized as a regular drug for home treatment of Covid-19. However, long-term abuse can lead to the accumulation of their toxic metabolites in the human body, which can easily cause cardiovascular disease and liver and kidney damage. Improper disposal and excessive discharge can enter environmental water sources and become common persistent organic pollutants in drinking water and surface water, endangering the health of aquatic organisms. Therefore, the establishment of a rapid and effective detection method for nonsteroidal anti-inflammatory drugs is of great significance to the sustainable development of the ecological environment.
[0003] Compared with traditional analytical methods, electrochemical sensing technology has shown great potential in the detection of organic pollutants due to its fast response, simple operation, low cost, high sensitivity and good selectivity.
[0004] Chinese patent CN114544720A discloses an electrochemical sensor for ultra-sensitive detection of enrofloxacin, which uses poly(p-aminobenzenesulfonic acid) and multi-walled carbon nanotube composite film to modify glassy carbon electrodes, showing high electrochemical response to enrofloxacin and achieving highly sensitive detection of enrofloxacin. Chinese patent CN115508427A discloses a method for preparing an electrochemically modified electrode for detecting bisphenol A in food, in which a silicon dioxide / indium tin oxide composite material is prepared by a solution growth method, a polydimethylsiloxane layer is deposited on the surface of the silicon dioxide / indium tin oxide composite material, and a uPS@SNCM / ITO electrochemically modified electrode is prepared for detecting bisphenol A in ethanol.
[0005] It can be seen that the detection performance of electrochemical sensors depends largely on the design and development of electrode materials. In recent years, transition metal selenides have shown great advantages in pollutant detection due to their rich redox sites, unique d-electron properties and chemical stability. In particular, bimetallic selenides have better synergistic effects and more mixed valence states, can provide richer electrochemical reactions, enhance charge transfer between different ions on the electrolyte and electrode surface, and show superior electrochemical performance.
[0006] Chinese patent CN114715857A discloses a method for preparing a bimetallic nickel-molybdenum-selenide electrode material, which obtains a nickel-molybdenum precursor by hydrothermal reaction, and calcines it with selenium powder in the heating zone of a tubular furnace to obtain a nickel-molybdenum-selenide with high conductivity and specific capacity. Chinese patent CN114525546A discloses a method for preparing a binary nickel-cobalt-selenide nanosheet material, and the binary nickel-cobalt-selenide nanosheet material obtained has a large specific surface area and high conductivity, and when used as an electrocatalytic material for oxygen evolution reaction, the electrochemical performance is greatly improved.
[0007] From the above background, it can be seen that bimetallic selenides have excellent application prospects in the field of electrochemistry. However, the practical application of single selenides still faces problems such as limited active sites and unsatisfactory conductivity. It is necessary to further develop electrode materials with good conductivity, multiple active sites and good electrocatalytic performance for the detection of non-steroidal anti-inflammatory drugs. Summary of the invention
[0008] The purpose of the present invention is to solve the problem that the existing single selenide is still faced with limited active sites and unsatisfactory conductivity in the field of electrochemistry, and it is necessary to develop a simple, fast, low-cost and highly sensitive electrochemical sensor for detecting non-steroidal anti-inflammatory drugs. A preparation method of a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material and its application are provided.
[0009] The present invention discloses a method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material (N-FeCoSe / CNTs) composite electrode material. A bimetallic organic framework (MOFs) material is used as a precursor. The N-FeCoSe / CNTs composite material is prepared by morphology control, electronegative heteroatom doping, high-temperature selenization and other strategies. An electrochemical sensor is constructed to achieve sensitive detection of the non-steroidal anti-inflammatory drug ibuprofen (IB).
[0010] The method provided by the present invention can simultaneously realize the simultaneous integration of bimetallic selenides with heteroatoms and carbon nanotubes, and construct an electrochemical sensing platform to realize the effective detection of non-steroidal anti-inflammatory drugs, which has important research significance and practical application value.
[0011] A method for preparing a nitrogen-doped iron-cobalt-selenide / carbon nanotube composite electrode material is specifically completed by the following steps:
[0012] 1. Add FeCl3·6H2O, Co(NO3)2·6H2O and terephthalic acid into a certain volume of N,N-dimethylformamide and stir until completely dissolved to obtain a mixed solution I;
[0013] 2. Add a certain amount of benzimidazole to the above mixed solution and stir for a period of time to obtain mixed solution II;
[0014] 3. Pour the mixed solution II into a high-pressure reactor, heat it to a certain temperature, heat it at a certain temperature for a period of time, wait for the reactor to cool to room temperature, pour out the supernatant, collect the precipitate by centrifugation, wash and dry it to obtain orange FeCo-MOFs powder;
[0015] Fourth, the FeCo-MOFs powder is placed in a tubular furnace, a selenium source is placed upstream of the tubular furnace, the temperature is raised to a calcination temperature under an inert gas atmosphere, and calcined at the calcination temperature for a period of time to obtain an N-FeCoSe / CNTs composite material, which is a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material.
[0016] A nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is used as an electrode material to construct an electrochemical sensor for use in the detection of non-steroidal anti-inflammatory drugs.
[0017] Advantages of the present invention:
[0018] (1) The present invention proposes a method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material, which is simple to prepare, low in cost, and environmentally friendly;
[0019] (2) In the present invention, nitrogen atom doping and carbon nanotube conversion are simultaneously achieved during the precursor selenization calcination process. Controllable nitrogen atom doping can directly affect the morphology and size of the material, thereby affecting its electrochemical properties;
[0020] (3) The nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material prepared by the present invention has rich porosity, good conductivity, more electroactive sites and fast charge transfer paths, and is suitable for constructing electrochemical sensors;
[0021] (4) In the present invention, the transition metal sites in the bimetallic selenide facilitate the attachment of organic functional groups on the electrode surface, thereby increasing the enrichment of ibuprofen (IB) on the electrode surface. The carbon nanotubes promote the charge transfer between IB and the electrode. The nitrogen atom doping synergistically enhances the electrochemical oxidation of ibuprofen (IB), which can be applied to the effective detection of ibuprofen (IB).
[0022] The invention can obtain a nitrogen-doped iron-cobalt-selenide / carbon nanotube composite electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 (a) is a SEM image of the FeCo-MOFs powder prepared in step 3 of Example 1. Figure 1 (b) is a SEM image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 1;
[0024] Figure 2(a) is a SEM image of the FeCo-MOFs powder prepared in step 3 of Example 2. Figure 2 (b) is a SEM image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 2;
[0025] Figure 3 (a) is the SEM image of the FeCo-MOFs powder prepared in step 3 of control example 1. Figure 3 (b) is a SEM image of the FeCoSe / CNTs composite material prepared in step 4 of control example 1;
[0026] Figure 4 XRD patterns of the composite materials prepared in step 4 of Example 1, Example 2 and Comparative Example 1;
[0027] Figure 5 (a) is the XPS image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 1. Figure 5 (b) is the XPS image of the FeCoSe / CNTs composite material prepared in step 4 of control example 1;
[0028] Figure 6 : is the differential pulse voltammetry curve of the electrode in the phosphate buffer solution of IB, in which a is the N-FeCoSe / CNTs modified electrode obtained in Example 3, b is the FeCoSe / CNTs modified electrode obtained in Control Example 2, and c is the bare electrode;
[0029] Figure 7 The differential pulse voltammograms of different concentrations of IB on the obtained N-FeCoSe / CNTs modified electrode in Example 3. DETAILED DESCRIPTION
[0030] Specific implementation method 1: This implementation method is a method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material, which is specifically completed by the following steps:
[0031] 1. Add FeCl3·6H2O, Co(NO3)2·6H2O and terephthalic acid into a certain volume of N,N-dimethylformamide and stir until completely dissolved to obtain a mixed solution I;
[0032] 2. Add a certain amount of benzimidazole to the above mixed solution and stir for a period of time to obtain mixed solution II;
[0033] 3. Pour the mixed solution II into a high-pressure reactor, heat it to a certain temperature, heat it at a certain temperature for a period of time, wait for the reactor to cool to room temperature, pour out the supernatant, collect the precipitate by centrifugation, wash and dry it to obtain orange FeCo-MOFs powder;
[0034] Fourth, the FeCo-MOFs powder is placed in a tubular furnace, a selenium source is placed upstream of the tubular furnace, the temperature is raised to a calcination temperature under an inert gas atmosphere, and calcined at the calcination temperature for a period of time to obtain an N-FeCoSe / CNTs composite material, which is a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material.
[0035] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the sum of the amounts of FeCl3·6H2O and Co(NO3)2·6H2O described in step 1 is equal to the amount of terephthalic acid; the molar volume ratio of FeCl3·6H2O, terephthalic acid and N,N-dimethylformamide described in step 1 is (1mmol~1.5mmol):2mmol:(20mL~30mL). The other steps are the same as those in specific embodiment 1.
[0036] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the molar ratio of the benzimidazole in step 2 to the terephthalic acid in step 1 is (0.5 mmol to 1.5 mmol): 2 mmol; the stirring time in step 2 is 20 min to 30 min. The other steps are the same as those in specific embodiment 1 or 2.
[0037] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the heating rate in step 3 is 5°C / min to 10°C / min; heating is performed at 100°C to 120°C for 15h to 24h in step 3. The other steps are the same as those in specific embodiments 1 to 3.
[0038] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the number of centrifugal revolutions in step 3 is 4000 rpm to 8000 rpm, and the centrifugal time is 5 min to 10 min; the washing solvents in step 3 are DMF and anhydrous ethanol, and the number of washings is 3 to 5 times; the drying temperature in step 3 is 60° C. to 80° C., and the drying time is 6 h to 12 h. The other steps are the same as those in specific embodiments 1 to 4.
[0039] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the selenium source in step 4 is selenium powder; the mass ratio of FeCo-MOFs powder to selenium source in step 4 is 1:3. The other steps are the same as those in specific embodiments 1 to 5.
[0040] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the inert gas in step 4 is nitrogen or argon, and the calcination temperature in step 4 is 450° C. to 650° C. The other steps are the same as those in specific embodiments 1 to 6.
[0041] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the calcination time in step 4 is 1 h to 3 h, and the heating rate in step 4 is 2°C / min to 5°C / min. The other steps are the same as those in specific embodiments 1 to 7.
[0042] Specific implementation method 9: This implementation method is to use a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material as an electrode material to construct an electrochemical sensor for use in the detection of non-steroidal anti-inflammatory drugs.
[0043] Specific implementation method 10: This implementation method is different from specific implementation methods 1 to 9 in that: the application method is as follows:
[0044] A nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is ultrasonically dispersed in deionized water to form a dispersion liquid, and the dispersion liquid is droplet-coated on a glassy carbon electrode as a working electrode, a platinum wire as a counter electrode, and a saturated calomel electrode as a reference electrode. The dispersion liquid is then placed in an electrolytic cell to form a three-electrode system. Differential pulse voltammetry is used to detect non-steroidal anti-inflammatory drug solutions of different concentrations in a phosphate buffer solution. The scanning potential range is 0.4V to 1.8V. The concentration of the non-steroidal anti-inflammatory drug solution is used as the horizontal coordinate and the peak current value is used as the vertical coordinate. The detection working curve is drawn to obtain the detection limit.
[0045] The concentration of the dispersion is 1 mg / mL to 3 mg / mL;
[0046] The volume of the dispersed liquid droplets applied on the glassy carbon electrode is 5 μL to 10 μL;
[0047] The nonsteroidal anti-inflammatory drug is ibuprofen;
[0048] The pH value of the phosphate buffer solution is 5-8;
[0049] The concentration of the non-steroidal anti-inflammatory drug solution is 1 μmol / L to 200 μmol / L. The other steps are the same as those of the first to ninth embodiments.
[0050] The following implementation is used to verify the beneficial effects of the present invention:
[0051] Example 1: A method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is specifically completed by the following steps:
[0052] 1. Add ferric chloride (FeCl3·6H2O), cobalt nitrate (Co(NO3)2·6H2O) and terephthalic acid (H2BDC) into a certain volume of N,N-dimethylformamide (DMF), stir until completely dissolved, and obtain a mixed solution I;
[0053] The molar volume ratio of FeCl3·6H2O, Co(NO3)2·6H2O, terephthalic acid and N,N-dimethylformamide described in step 1 is 1.5mmol:0.5mmol:2mmol:30mL;
[0054] 2. Add 0.6 mmol of benzimidazole to the above mixed solution and stir for 30 min to obtain mixed solution II;
[0055] 3. Pour the mixed solution II into a high-pressure reactor, heat it to 110°C at a heating rate of 10°C / min, heat it at 110°C for 15h, wait for the reactor to cool to room temperature, pour out the supernatant, collect the precipitate by centrifugation, wash the precipitate with DMF and anhydrous ethanol for 5 times respectively, and then dry it at 80°C for 8h to obtain orange FeCo-MOFs powder;
[0056] The centrifugal speed in step 3 is 4000 rpm;
[0057] The centrifugation time described in step 3 is 5 minutes;
[0058] Fourth, FeCo-MOFs powder is placed in a tubular furnace, a selenium source is placed upstream of the tubular furnace, the temperature is raised to a calcination temperature under an inert gas atmosphere, and calcined at the calcination temperature for a period of time to obtain a N-FeCoSe / CNTs composite material, i.e., a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material (N-FeCoSe / CNTs composite material);
[0059] The selenium source described in step 4 is selenium powder;
[0060] The mass ratio of the FeCo-MOFs powder to the selenium source described in step 4 is 1:3.
[0061] The inert gas described in step 4 is: nitrogen;
[0062] The calcination temperature in step 4 is: 650°C;
[0063] The calcination time in step 4 is: 2h;
[0064] The heating rate described in step 4 is 5°C / min.
[0065] Example 2: A method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is specifically completed by the following steps:
[0066] 1. Add ferric chloride (FeCl3·6H2O), cobalt nitrate (Co(NO3)2·6H2O) and terephthalic acid (H2BDC) into a certain volume of N,N-dimethylformamide (DMF), stir until completely dissolved, and obtain a mixed solution I;
[0067] The molar volume ratio of FeCl3·6H2O, Co(NO3)2·6H2O, terephthalic acid and N,N-dimethylformamide described in step 1 is 1mmol:1mmol:2mmol:30mL;
[0068] 2. Add 1.2 mmol of benzimidazole to the above mixed solution and stir for 30 minutes to obtain mixed solution II;
[0069] 3. Pour the mixed solution II into a high-pressure reactor, heat it to 100°C at a heating rate of 10°C / min, heat it at 100°C for 24 hours, wait for the reactor to cool to room temperature, pour out the supernatant, collect the precipitate by centrifugation, wash the precipitate three times with DMF and anhydrous ethanol respectively, and then dry it at 80°C for 10 hours to obtain orange FeCo-MOFs powder;
[0070] The centrifugal speed in step 3 is 4000 rpm;
[0071] The centrifugation time described in step 3 is 5 minutes;
[0072] Fourth, FeCo-MOFs powder is placed in a tubular furnace, a selenium source is placed upstream of the tubular furnace, the temperature is raised to a calcination temperature under an inert gas atmosphere, and calcined at the calcination temperature for a period of time to obtain a N-FeCoSe / CNTs composite material, i.e., a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material (N-FeCoSe / CNTs composite material);
[0073] The selenium source described in step 4 is selenium powder;
[0074] The mass ratio of the FeCo-MOFs powder to the selenium source described in step 4 is 1:3.
[0075] The inert gas described in step 4 is: nitrogen;
[0076] The calcination temperature in step 4 is: 600°C;
[0077] The calcination time in step 4 is: 2h;
[0078] The heating rate described in step 4 is 5°C / min.
[0079] Comparative Example 1: The difference between this comparative example and Example 1 is that in step 2, 0 mmol of benzimidazole is added to the mixed solution and stirred for 30 min to obtain a mixed solution II. The other steps and parameters are the same as those in Example 1, and finally an iron cobalt selenide / carbon nanotube composite electrode material (FeCoSe / CNTs composite material) is obtained.
[0080] Example 3: Using a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material prepared in Example 1 as an electrode material to construct an electrochemical sensor for use in the detection of nonsteroidal anti-inflammatory drugs, the application method is as follows:
[0081] 3 mg of a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material prepared in Example 1 was ultrasonically dispersed in 1 mL of deionized water to form a dispersion liquid, 8 μL of the dispersion liquid was dropleted using a pipette and applied to the surface of a glassy carbon electrode, and dried under an infrared lamp to form a uniform film to obtain an N-FeCoSe / CNTs modified electrode, which was used as a working electrode, a platinum wire as a counter electrode, and a saturated calomel electrode as a reference electrode, and then placed in an electrolytic cell to form a three-electrode system; the three-electrode system was placed in an electrolytic cell containing a phosphate buffer solution with a concentration of 0.1 mol / L and a pH of 7 to construct an electrochemical sensor; ibuprofen (IB) standard solutions of different concentrations were accurately added to the electrolytic cell using a pipette, and ibuprofen (IB) was detected by differential pulse voltammetry, with a scanning potential interval of 0.4-1.8 V, the IB concentration as the horizontal axis, and the peak current value as the vertical axis, and a detection working curve was plotted to obtain the detection limit.
[0082] The concentration of the non-steroidal anti-inflammatory drug solution is 1 μmol / L to 200 μmol / L.
[0083] Control Example 2: The difference between this control example and Example 3 is that 3 mg of the iron cobalt selenide / carbon nanotube composite electrode material (FeCoSe / CNTs composite material) prepared in Control Example 1 is ultrasonically dispersed in 1 mL of deionized water to form a dispersion, and the other steps and parameters are the same as those in Example 1, recorded as FeCoSe / CNTs modified electrode.
[0084] Figure 1 (a) is a SEM image of the FeCo-MOFs powder prepared in step 3 of Example 1. Figure 1 (b) is a SEM image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 1;
[0085] like Figure 1 As shown in (a): When the amount of benzimidazole added is 0.6 mmol, the obtained FeCo-MOFs precursor exhibits a spindle-like morphology with an average size of 1.5 μm and a width of 300 nm. Figure 1It can be seen in (b) that after high-temperature calcination, the spindle rod size shrinks slightly, the surface becomes rough and porous, and is converted into bimetallic iron cobalt selenide. In addition, with the high-temperature volatilization of organic ligands, many carbon nanotube structures are formed.
[0086] Figure 2 (a) is a SEM image of the FeCo-MOFs powder prepared in step 3 of Example 2. Figure 2 (b) is a SEM image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 2;
[0087] like Figure 2 As shown in (a): When the amount of benzimidazole added is increased to 1.2mmol, the FeCo-MOFs precursor obtained presents a rod-like morphology and begins to shrink in size, with an average size of 500nm and a width of 150nm, indicating that the amount of benzimidazole added can directly affect the morphology and size of the material. Figure 2 As can be seen in (b), the material morphology becomes irregular after high-temperature calcination, but the carbon nanotube structure can still be observed.
[0088] Figure 3 (a) is the SEM image of the FeCo-MOFs powder prepared in step 3 of control example 1. Figure 3 (b) is a SEM image of the FeCoSe / CNTs composite material prepared in step 4 of control example 1;
[0089] like Figure 3 As shown in (a): When the amount of benzimidazole added is 0 mmol, the original FeCo-MOFs precursor obtained is a three-dimensional spherical morphology with an average diameter of 700 nm, which further illustrates that the addition of benzimidazole can adjust the material morphology and is the key to obtaining a rod-shaped FeCo-MOFs precursor. Figure 2 As can be seen in (b), the spherical morphology collapses after high-temperature calcination, and some irregular blocks can be observed to be staggered with carbon nanotubes.
[0090] Figure 4 XRD patterns of the composite materials prepared in step 4 of Example 1, Example 2 and Comparative Example 1;
[0091] Depend on Figure 4 It can be seen that the diffraction peaks at 2θ=33.2°, 33.8°, 43.9°, 44.8°, 51.5° and 63.1° are attributed to the (-112), (202), (-114), (114), (020) and (222) crystal planes of Fe2CoSe4 (JCPDS card No.89-1967). A broad peak appears at 24°, corresponding to the (002) crystal plane of graphite carbon. This shows that Example 1, Example 2 and Comparative Example 1 successfully prepared the iron cobalt selenide / carbon nanotube composite material.
[0092] Figure 5 (a) is the XPS image of the N-FeCoSe / CNTs composite material prepared in step 4 of Example 1. Figure 5 (b) is the XPS image of the FeCoSe / CNTs composite material prepared in step 4 of control example 1;
[0093] Figure 5 (a) Confirmed the presence of Co, Fe, Se, O and N elements in the prepared N-FeCoSe / CNTs composites, while Figure 5 The N1s signal was not detected in (b), further confirming the role of benzimidazole as a nitrogen dopant in the present invention.
[0094] Figure 6 : is the differential pulse voltammetry curve of the electrode in the phosphate buffer solution of IB, in which a is the N-FeCoSe / CNTs modified electrode obtained in Example 3, b is the FeCoSe / CNTs modified electrode obtained in Control Example 2, and c is the bare electrode;
[0095] In a phosphate buffer solution with a pH of 7, the electrochemical signals of 100 μmol / L IB on N-FeCoSe / CNTs modified electrode, FeCoSe / CNTs modified electrode and bare electrode were compared by differential pulse voltammetry. In the scanning range of 0.4-1.8V, IB showed only a weak oxidation peak on the bare electrode, and on the FeCoSe / CNTs modified electrode, the peak current of IB increased, indicating that the FeCoSe / CNTs material has good electrocatalytic properties. On the N-FeCoSe / CNTs modified electrode, the peak current of IB doubled, indicating that the introduction of nitrogen elements in the structure further enhances the conductivity of the material, provides more electroactive sites, and exhibits a better detection ability for IB.
[0096] Figure 7 The differential pulse voltammograms of different concentrations of IB on the obtained N-FeCoSe / CNTs modified electrode in Example 3;
[0097] from Figure 7 It can be seen that as the IB concentration increases, the peak current also increases, and there is an obvious two-segment linear relationship. From the concentration range of 1-20μmol / L, the linear equation is: I pa =4.909c+9.229(R 2 =0.991), in the concentration range of 20-200 μmol / L, the linear equation is: pa =1.161c+88.305(R 2=0.997), with a detection limit of 0.3 μmol / L, achieving effective detection of IB, confirming the feasibility of the nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material proposed in the present invention in detecting non-steroidal anti-inflammatory drugs.
Claims
1. A method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material, characterized in that The preparation method is specifically completed according to the following steps:
1. Add FeCl3·6H2O, Co(NO3)2·6H2O and terephthalic acid into a certain volume of N,N-dimethylformamide and stir until completely dissolved to obtain a mixed solution I; The sum of the amounts of FeCl3·6H2O and Co(NO3)2·6H2O described in step 1 is equal to the amount of terephthalic acid; the molar volume ratio of FeCl3·6H2O, terephthalic acid and N,N-dimethylformamide described in step 1 is (1mmol-1.5mmol):2mmol:(20mL-30mL); 2. Add a certain amount of benzimidazole to the above mixed solution and stir for a period of time to obtain mixed solution II; The molar ratio of the benzimidazole in step 2 to the terephthalic acid in step 1 is (0.5mmol-1.5mmol):2mmol; the stirring time in step 2 is 20min-30min; 3. Pour the mixed solution II into a high-pressure reactor, heat it to a certain temperature, heat it at a certain temperature for a period of time, wait for the reactor to cool to room temperature, pour out the supernatant, collect the precipitate by centrifugation, wash and dry it to obtain orange FeCo-MOFs powder; The heating rate in step 3 is 5°C / min to 10°C / min; heating at 100°C to 120°C for 15h to 24h in step 3; Fourth, the FeCo-MOFs powder is placed in a tubular furnace, a selenium source is placed upstream of the tubular furnace, the temperature is raised to a calcination temperature under an inert gas atmosphere, and calcined at the calcination temperature for a period of time to obtain an N-FeCoSe / CNTs composite material, which is a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material.
2. The method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material according to claim 1, characterized in that The number of centrifuge revolutions in step three is 4000 rpm to 8000 rpm, and the centrifugation time is 5 min to 10 min; the washing solvents in step three are DMF and anhydrous ethanol, and the number of washings is 3 to 5 times; the drying temperature in step three is 60° C. to 80° C., and the drying time is 6 h to 12 h.
3. The method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material according to claim 1, characterized in that The selenium source described in step 4 is selenium powder; the mass ratio of the FeCo-MOFs powder and the selenium source described in step 4 is 1:
3.
4. The method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material according to claim 1, characterized in that The inert gas described in step 4 is nitrogen or argon; the calcination temperature described in step 4 is 450°C to 650°C.
5. The method for preparing a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material according to claim 1, characterized in that The calcination time in step 4 is 1 h to 3 h; the heating rate in step 4 is 2° C. / min to 5° C. / min.
6. Use of a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material prepared by the preparation method according to claim 1, characterized in that A nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is used as an electrode material to construct an electrochemical sensor for use in the detection of non-steroidal anti-inflammatory drugs.
7. The use of a nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material according to claim 6, characterized in that The application method is as follows: A nitrogen-doped iron cobalt selenide / carbon nanotube composite electrode material is ultrasonically dispersed in deionized water to form a dispersion liquid, and the dispersion liquid is droplet-coated on a glassy carbon electrode as a working electrode, a platinum wire as a counter electrode, and a saturated calomel electrode as a reference electrode. The dispersion liquid is then placed in an electrolytic cell to form a three-electrode system. Differential pulse voltammetry is used to detect non-steroidal anti-inflammatory drug solutions of different concentrations in a phosphate buffer solution. The scanning potential range is 0.4V to 1.8V. The concentration of the non-steroidal anti-inflammatory drug solution is used as the horizontal coordinate and the peak current value is used as the vertical coordinate. The detection working curve is drawn to obtain the detection limit. The concentration of the dispersion is 1 mg / mL to 3 mg / mL; The volume of the dispersed liquid droplets applied on the glassy carbon electrode is 5 μL to 10 μL; The nonsteroidal anti-inflammatory drug is ibuprofen; The pH value of the phosphate buffer solution is 5-8; The concentration of the non-steroidal anti-inflammatory drug solution is 1 μmol / L to 200 μmol / L.