A micro-nano patterning preparation method of a semiconductor and an optoelectronic imaging device
By growing AgBiS2 on a SiO2 substrate using a silver oxide seed layer, bottom-up nanomaterial patterning was achieved, solving the problems of high cost, complex process, and etching contamination in existing technologies, and a high-resolution optoelectronic imaging device was fabricated.
Patent Information
- Application Number
- CN202410093772.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-23
AI Technical Summary
Existing methods for patterning nanomaterials are costly and complex, and the etching process introduces surface contamination that affects material quality, making it difficult to achieve high-resolution patterning.
A bottom-up additive manufacturing method is adopted to grow AgBiS2 using a silver oxide seed layer on the surface of a SiO2 substrate. Patterned growth is achieved on any substrate through photolithography and spin coating, avoiding surface contamination introduced by the etching process.
This method enables simple and rapid patterned growth of nanomaterials on any substrate, avoiding contamination from the etching process, and fabricates a high-resolution multi-pixel dot array image sensor, solving the problems of low resolution and unclear pattern edges in traditional methods.
Smart Images

Figure CN117936645B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photoelectric detection technology, specifically to a method for fabricating micro-nano patterned semiconductors and a photoelectric imaging device. Background Technology
[0002] Patterning is the core of semiconductor microelectronic device manufacturing processes. Taking silicon as an example, the main approach is a top-down "growth and etching" route, where photolithography is used to subtract material from the semiconductor to achieve micro / nano patterning. Decades of technological advancements have enabled nanoscale patterning in semiconductor manufacturing processes. However, the stringent process requirements impose cost and technological constraints, and the etching process negatively impacts the electrical properties of semiconductors, hindering the future development of smaller, higher-performance microelectronics and integrated circuits. Therefore, breaking through the limitations of traditional semiconductor processes and inventing a bottom-up additive manufacturing micro / nano patterning process that avoids the adverse effects of subtractive etching is of great significance.
[0003] On the other hand, low-dimensional materials, represented by nanowires, and their self-assembled three-dimensional structures possess unique optical and electrical properties due to their distinctive structural characteristics and surface effects. This allows them to overcome the performance limitations of traditional silicon-based and thin-film microelectronic devices at the material level, showing significant potential, especially in photoelectric detection and imaging applications. Therefore, research on the patterned fabrication of photosensitive semiconductor nanostructures is crucial for next-generation optoelectronic devices. Currently, many nanoassembly strategies have been developed, including post-synthesis assembly and in-situ epitaxial growth, to address scalability and integrability issues by configuring large-scale crystalline nanowires in parallel or random network thin films. Post-synthesis assembly, such as contact printing and liquid phase deposition, is commonly used to assemble nanowires into high-performance electronic and optoelectronic devices; for example, hydrophilic and hydrophobic substrates are prepared using microcontact imprinting, followed by selective substrate formation of zirconia nanoparticles to obtain zirconia particle microarrays. In-situ epitaxial growth bypasses the complex two-part assembly process, allowing for bottom-up research on materials and exploration of their functional devices. For example, in some cases, gallium nitride nanowires with controllable crystal orientation are grown on specific crystal faces of sapphire. Furthermore, the patterning of nanomaterials can also be achieved using a top-down "growth and etching" approach similar to silicon-based processes. This involves subtractive manufacturing followed by etching away unwanted portions to pattern the nanomaterials. For example, electron beam lithography has been used to fabricate microarrays of platinum nanoparticles on the surface of silicon wafers.
[0004] AgBiS2 is an environmentally friendly IV-VI2 group ternary semiconductor material with a broad absorption spectrum (300-1600 nm) in the visible to near-infrared region, extremely high light absorption coefficient, and the ability to overcome the spectral absorption limitations of silicon-based devices in the short-wave infrared region, showing great application potential in the field of photoelectric detection. Currently, AgBiS2 optoelectronic device technology is limited to nanoparticle sol-film methods; there are no reports on the micro / nano patterning fabrication and imaging applications of this novel semiconductor.
[0005] The assembly methods for synthesized nanomaterials are costly and complex, and are selective in terms of materials and substrates, making it difficult to achieve high-resolution patterning. In-situ epitaxial growth always involves high growth temperatures, strict requirements for atomic planes and multiplanar substrates, and heteroepitaxial relationships, which significantly increases the complexity of material processing. The top-down "growth and etching" route increases the complexity of the process, and surface contamination introduced by the etching process can affect the quality of nanomaterials.
[0006] Therefore, it is necessary to find suitable materials and growth strategies to address the challenges currently faced in the patterning fabrication of nano-semiconductor materials. Summary of the Invention
[0007] In view of this, the present invention provides a method for fabricating micro-nano patterned semiconductors and an optoelectronic imaging device, which can realize patterned growth on various substrates. The growth depends only on the seed layer on the substrate surface. The fabrication method is simple, convenient and fast, and at the same time, it can avoid the surface contamination introduced by the etching process from affecting the quality of the grown nanomaterials.
[0008] To achieve the above objectives, the present invention provides a method for fabricating micro / nano patterned semiconductors, comprising the following steps: S100, cleaning SiO2 substrate.
[0009] S200, a micron-scale linear array pattern is formed on a cleaned SiO2 substrate by photolithography.
[0010] S300 involves depositing nanometer-thick silver onto a photolithographically patterned SiO2 substrate to remove residual photoresist from the SiO2.
[0011] S400 involves placing a SiO2 substrate coated with nano-silver in a plasma cleaner to oxidize the silver on its surface into silver oxide.
[0012] S500 involves spin-coating an AgBiS2 solution onto a SiO2 substrate containing silver oxide, annealing it at a certain temperature for a certain time, and repeating this step three times to obtain a micro / nano patterned semiconductor on a SiO2 substrate.
[0013] Preferably, in step S100, the SiO2 substrate is cleaned by sequentially ultrasonically cleaning it with acetone, water, and ethanol for 30 minutes.
[0014] Preferably, in step S200, a micron-scale linear array pattern is formed on a cleaned SiO2 substrate by photolithography, wherein the photolithography process includes spin coating, pre-baking, exposure and development steps, and the micron-scale linear array pattern is formed on the cleaned SiO2 substrate by photolithography.
[0015] Furthermore, in S300, a nanometer-thick layer of silver is deposited on a photolithographically patterned SiO2 substrate to remove residual photoresist from the SiO2. Specifically, a 10-nanometer layer of silver is deposited on the photolithographically patterned SiO2 substrate using a thermal evaporation deposition apparatus. Then, the substrate is immersed in a photoresist remover solution to remove residual photoresist from the substrate, thereby forming a silver micron array pattern on the SiO2 substrate.
[0016] Preferably, in step S400, the SiO2 substrate coated with nano-silver is placed in a plasma cleaner to oxidize the silver on its surface into silver oxide. Specifically, the oxygen flow rate in the plasma cleaner is set to 5 sccm, and the silver oxide on the surface of the SiO2 substrate acts as a seed layer to participate in the reaction. That is, AgBiS2 will grow where there is a silver oxide seed layer, and AgBiS2 will not grow where there is no silver oxide seed layer, thereby realizing the patterned growth of AgBiS2 material.
[0017] Preferably, the AgBiS2 solution is prepared as follows: AgCl, BiCl3, and thiourea are weighed and dissolved in N,N-dimethylformamide solution, and stirred to mix evenly, wherein the concentration ratio is Ag:Bi:thiourea = 1:1:1.8; the SiO2 substrate with a patterned silver oxide seed layer is placed in a spin coater and rotated at a speed of not less than 2500 rpm for 60 seconds. During the rotation, the evenly mixed AgBiS2 solution is added dropwise onto the SiO2 substrate to achieve spin coating. Then, it is heated in the range of 170-240 degrees Celsius for 5-10 minutes to achieve heating; the "spin coating-heating" process is repeated three times to obtain micro-nano patterned AgBiS2 semiconductors on the SiO2 substrate.
[0018] Another embodiment of the present invention provides a photoelectric imaging device fabricated by micro-nano patterning of semiconductors, including: a SiO2 substrate, an AgBiS2 linear array, and gold electrodes covering the AgBiS2 linear array.
[0019] The above-mentioned semiconductor micro-nano patterning fabrication method was used to fabricate an AgBiS2 linear array on a SiO2 substrate.
[0020] The linewidth of the AgBiS2 linear array is no higher than 20 micrometers, and the line spacing is no higher than 30 micrometers.
[0021] Multiple gold electrodes are vertically arranged above the AgBiS2 linear array, with the distance between adjacent gold electrodes not exceeding 100 micrometers, and the thickness of the gold electrodes being between 50 and 100 nanometers.
[0022] Preferably, the AgBiS2 linear array has a line spacing of 20 micrometers and a line width of 10 micrometers.
[0023] Preferably, the distance between each pair of gold electrodes is 50 micrometers, and each pair of gold electrodes and the linear array between them constitute a device; each device contains 16 linear arrays.
[0024] Preferably, gold electrodes are deposited on the neatly arranged AgBiS2 linear array using a thermal evaporation method, and the thickness of the gold electrodes is 50 nanometers.
[0025] Beneficial effects: 1. The present invention provides a method for fabricating micro-nano patterned semiconductors, which can achieve growth on any substrate and overcome substrate selectivity. In the micro-nano patterned fabrication method provided by the present invention, the growth of AgBiS2 mainly depends on the silver oxide seed layer on the substrate surface. That is, AgBiS2 only grows where there is a silver oxide seed layer, and AgBiS2 will not grow where there is no silver oxide seed layer. Thus, patterned growth on any substrate can be achieved. Its growth depends only on the seed layer on the substrate surface. The fabrication method is simple, convenient and fast.
[0026] 2: The present invention provides a semiconductor micro / nano patterning fabrication method, which is a bottom-up patterning fabrication method. The fabrication method is simple, convenient, fast, and low in cost. At the same time, it can avoid the problems of surface contamination and time consumption introduced by the top-down etching process. The present invention provides a bottom-up additive manufacturing patterning fabrication method, which realizes arbitrary patterned growth of AgBiS2 on the substrate by means of a silver oxide seed layer. This overcomes the substrate selectivity of material growth and avoids the surface contamination introduced by the etching process from affecting the quality of the grown nanomaterials.
[0027] 3. This invention provides a photoelectric imaging device fabricated using micro- and nano-patterning of semiconductors. The devices fabricated using the patterning method are independent of each other, making it possible to fabricate large-scale, low-crosstalk, multi-pixel array image sensors. The patterning method for photosensitive semiconductors provided by this invention can achieve micrometer-level resolution, solving the problems of low resolution and unclear pattern edges inherent in traditional patterning methods. Attached Figure Description
[0028] Figure 1This is a schematic diagram of a semiconductor micro / nano patterning fabrication method provided in Embodiment 1 of the present invention; wherein 1-SiO2 substrate; 2-silver micron array pattern; 3-AgBiS2 droplets; 4-AgBiS2 self-assembled multi-level flower structure; 5-gold electrode array; Figure 2 This is a partial schematic diagram of a regularly arranged AgBiS2 linear array in an image sensor based on micro-nano patterned semiconductors under a scanning electron microscope. Figure 3 This is a schematic diagram of AgBiS2 material with "goldfish", "panda" and "cherry" patterns prepared by a semiconductor micro-nano patterning preparation method provided in Example 1. Figure 4 This is a scanning electron microscope characterization image based on a single-wire micro-nano patterned optoelectronic imaging device; Figure 5 (A) is a graph showing the change of photocurrent over time at different wavelengths of an optoelectronic imaging device based on single-wire micro-nano patterning provided in an embodiment of the present invention. Figure 5 (B) is a graph showing the change of photocurrent over time under different optical powers when a photoelectric imaging device based on single-wire micro-nano patterning is irradiated by a 520 nm laser, according to an embodiment of the present invention. Figure 6 A schematic diagram of a micro-nano patterned photoelectric imaging device provided in an embodiment of the present invention; Figure 7 The illustration shows a schematic diagram of an optoelectronic imaging device fabricated using micro-nano patterning, provided by an embodiment of the present invention. Detailed Implementation
[0029] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0030] Example 1 Figure 1 This illustration schematically depicts a method for fabricating micro / nano patterned semiconductors according to an embodiment of the present invention. For example... Figure 1 As shown, the semiconductor micro / nano patterning fabrication method provided in this embodiment of the invention includes steps S100-S400.
[0031] S100, cleaning SiO2 substrate 1.
[0032] In an embodiment of the present invention, the SiO2 substrate was ultrasonically cleaned for 30 minutes in sequence with acetone, water, and acetone.
[0033] S200 is a micron-scale linear array pattern formed by photolithography on a SiO2 substrate.
[0034] The photolithography process includes steps such as spin coating, pre-baking, exposure, and development, and photolithographic micron-scale patterns are formed on a cleaned SiO2 substrate.
[0035] S300 involves depositing nanometer-thick silver onto a photolithographically patterned SiO2 substrate to remove residual photoresist from the SiO2.
[0036] In this embodiment of the invention, a thermal evaporation deposition apparatus is used to deposit 10 nanometers of silver on a photolithographically patterned SiO2 substrate. Then, the substrate is immersed in a photoresist remover to remove the residual photoresist on the substrate, thereby forming a silver micron array pattern 2 on the SiO2 substrate.
[0037] S400: A SiO2 substrate coated with 10 nanometers of silver is placed in a plasma cleaner for 30 minutes to oxidize the silver on its surface into silver oxide.
[0038] The oxygen flow rate in the plasma cleaner is 5 sccm. In this embodiment of the invention, silver oxide on the surface of the SiO2 substrate serves as a seed layer to participate in the reaction. That is, AgBiS2 will grow where there is a silver oxide seed layer, and AgBiS2 will not grow where there is no silver oxide seed layer, thereby achieving patterned growth of AgBiS2 material.
[0039] S500 involves spin-coating an AgBiS2 solution onto a SiO2 substrate containing silver oxide, annealing it at a certain temperature for a certain time, and repeating this step three times to obtain a micro / nano patterned semiconductor on a SiO2 substrate.
[0040] In this embodiment of the invention, AgBiS2 solution 3 is spin-coated onto a SiO2 substrate containing silver oxide, annealed at 200°C for 5 minutes, and this step is repeated three times to obtain a micro-nano patterned semiconductor 4 on a SiO2 substrate.
[0041] AgCl, BiCl3, and thiourea were weighed and dissolved in N,N-dimethylformamide solution, and stirred until homogeneous, with a concentration ratio of Ag:Bi:thiourea = 1:1:1.8. In this embodiment, 0.3583 g of AgCl, 0.68835 g of BiCl3, and 1.37016 g of thiourea were weighed and dissolved in 10 mL of N,N-dimethylformamide solution, and stirred for 30 minutes until homogeneous. A SiO2 substrate with a patterned silver oxide seed layer was placed in a spin coater and rotated at a speed of at least 2500 rpm for 60 seconds (3000 rpm for 60 seconds in this embodiment). During rotation, one drop (50 μL) of the homogeneously mixed AgBiS2 solution was added to the SiO2 substrate. The substrate was then heated at 170-240°C for 5-10 minutes (200°C for 5 minutes in this embodiment). The spin-coating-heating process was repeated three times to obtain micro / nano-patterned AgBiS2 semiconductors on the SiO2 substrate.
[0042] Figure 2 yes Figure 1 A partial image of a regularly arranged AgBiS2 linear array in an image sensor based on micro-nano patterned semiconductors under a scanning electron microscope.
[0043] like Figure 2 As shown in (A), the AgBiS2 material exhibits a self-assembled, multi-level flower-like structure of nanowires. (As shown in the image...) Figure 2 As shown in (B), AgBiS2 exhibits patterned growth on the SiO2 substrate, meaning that AgBiS2 only grows where there is a silver oxide seed layer, and does not grow where there is no silver oxide seed layer. Patterned growth makes it possible to fabricate large-scale, low-crosstalk, multi-pixel dot array image sensors.
[0044] Figure 3 The AgBiS2 material with "goldfish", "panda" and "cherry" patterns was prepared using the semiconductor micro-nano patterning method provided in Example 1. The red box part is the scanning electron microscope characterization image of the corresponding part of the "goldfish" pattern. It can be seen that AgBiS2 can also exhibit other types of patterned growth on SiO2 substrate.
[0045] Example 2 like Figure 1 As shown, this embodiment of the invention also provides a photoelectric imaging device fabricated by micro-nano patterning, including: a SiO2 substrate 1; a regularly arranged AgBiS2 linear array 4; and gold electrodes 5 neatly arranged on the AgBiS2 array.
[0046] According to an embodiment of the present invention, a photoelectric imaging device fabricated by micro-nano patterning is provided, wherein the regularly arranged AgBiS2 linear array (ensuring pixel uniformity) has a line width of no more than 20 micrometers and a line spacing of no more than 30 micrometers.
[0047] According to an embodiment of the present invention, the distance between gold electrodes in a micro-nano patterned optoelectronic imaging device is no more than 100 micrometers, and the thickness of the gold electrodes is between 50 and 100 nanometers.
[0048] AgBiS2 is an environmentally friendly IV-VI2 group ternary semiconductor material with a broad absorption spectrum (300-1600 nm) in the visible to near-infrared region. In recent years, AgBiS2 has become a promising candidate material in the field of optoelectronics due to its high absorption coefficient, good charge transport properties, excellent stability, and low cost. Applying AgBiS2 to image sensors can solve problems such as poor device stability, the inability to mass-produce device arrays, and high cost. AgBiS2 exhibits visible to near-infrared photosensitive properties. When AgBiS2 is photoexcited, the absorption of photons causes a change in carrier concentration, i.e., the formation of non-equilibrium carriers, leading to a change in the material's conductivity.
[0049] Figure 4 This is a scanning electron microscope characterization image of an optoelectronic imaging device based on micro-nano patterning of a single wire.
[0050] like Figure 4 As shown, a photoelectric imaging device based on single-wire micro-nano patterning includes: a SiO2 substrate; a single AgBiS2 wire; and a gold electrode.
[0051] In detail, the embodiment of the present invention provides a single AgBiS2 line with a linewidth of 5 micrometers, a distance of 50 micrometers between gold electrodes, and a thickness of 50 nanometers in a single-line micro-nano patterned photosensitive semiconductor device.
[0052] Example 3 Figure 5 (A) is a photocurrent variation curve of a photoelectric imaging device based on single-wire micro-nano patterning provided in an embodiment of the present invention at different wavelengths.
[0053] like Figure 5 As shown in (A), under laser irradiation with wavelengths of 405 nm, 520 nm, 750 nm, 1060 nm and 1450 nm, the single-line micro-nano patterned photosensitive semiconductor device has a higher photoresponse to 520 nm laser.
[0054] Figure 5 (B) is a curve showing the change of photocurrent over time under different optical powers when a photoelectric imaging device based on micro-nano patterning of a single wire is irradiated by a 520 nm laser, according to an embodiment of the present invention.
[0055] like Figure 5 As shown in (B), under laser irradiation with a wavelength of 520 nm, the higher the optical power, the stronger the photoresponse of the device.
[0056] Example 4 Figure 6This invention provides an optoelectronic imaging device based on the micro-nano patterning fabrication of semiconductors. For example... Figure 6 As shown, an image sensor based on micro-nano patterned photosensitive semiconductors provided in this embodiment of the invention includes: a SiO2 substrate; an AgBiS2 linear array; and a gold electrode array.
[0057] In detail, the image sensor AgBiS2 linear array based on micro-nano patterned photosensitive semiconductor provided by the embodiments of the present invention has a line width of 10 micrometers, a line spacing of 20 micrometers, a distance between gold electrodes of 50 micrometers, and a gold electrode thickness of 50 nanometers.
[0058] Example 5 Figure 7 The illustration shows a schematic diagram of an optoelectronic imaging device fabricated using micro-nano patterning, provided by an embodiment of the present invention.
[0059] like Figure 7 As shown, the 336 pixels make the image clearer and the butterfly pattern more vivid and lifelike. The excellent imaging capability indicates that the optoelectronic imaging device prepared by micro-nano patterning provided in this embodiment of the invention has excellent image sensing capability.
[0060] In detail, the experiment involved fabricating a 12×28 micro-nano patterned photosensitive semiconductor photodetector array on a SiO2 substrate. A wavelength of 1342 nm and a power of 860.4 mW / cm² were used. 2 The laser is used to irradiate the area, and the dark current and photocurrent at 1V are recorded for each pixel. The ratio of these values is used as a detection signal.
[0061] In summary, the above are merely preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for fabricating micro / nano patterned semiconductors, characterized in that, Includes the following steps: S100, cleaning the SiO2 substrate; S200, a micron-scale linear array pattern is formed on the cleaned SiO2 substrate by photolithography; S300 involves depositing nanometer-thick silver on a photolithographically patterned SiO2 substrate to remove residual photoresist from the SiO2. S400 involves placing a SiO2 substrate coated with nano-silver in a plasma cleaner to oxidize the silver on its surface into silver oxide. S500 involves spin-coating an AgBiS2 solution onto a SiO2 substrate containing silver oxide, annealing it at a certain temperature for a certain time, and repeating this step three times to obtain a micro / nano patterned semiconductor on a SiO2 substrate.
2. The method for fabricating micro / nano patterned semiconductors as described in claim 1, characterized in that, S100, cleaning the SiO2 substrate, specifically involves sequentially ultrasonically cleaning the SiO2 substrate with acetone, water, and acetylene for 30 minutes.
3. The method for fabricating micro / nano patterned semiconductors as described in claim 1, characterized in that, In step S200, a micron-scale linear array pattern is formed on the cleaned SiO2 substrate by photolithography. The photolithography process includes spin coating, pre-baking, exposure, and development steps. The micron-scale linear array pattern is formed on the cleaned SiO2 substrate by photolithography.
4. The method for fabricating micro / nano patterned semiconductors as described in claim 1, characterized in that, In step S300, a nanometer-thick layer of silver is deposited on a photolithographically patterned SiO2 substrate to remove residual photoresist from the SiO2. Specifically, a 10-nanometer layer of silver is deposited on the photolithographically patterned SiO2 substrate using a thermal evaporation deposition apparatus. Then, the substrate is immersed in a photoresist remover solution to remove residual photoresist from the substrate, thereby forming a silver micron array pattern on the SiO2 substrate.
5. The method for fabricating micro / nano patterned semiconductors as described in claim 1, characterized in that, In step S400, the SiO2 substrate coated with nano-silver is placed in a plasma cleaner for treatment, causing the silver on its surface to oxidize into silver oxide. Specifically, the oxygen flow rate in the plasma cleaner is set to 5 sccm, and the silver oxide on the surface of the SiO2 substrate acts as a seed layer to participate in the reaction. That is, AgBiS2 will grow where there is a silver oxide seed layer, and AgBiS2 will not grow where there is no silver oxide seed layer, thereby realizing the patterned growth of AgBiS2 material.
6. The method for fabricating micro / nano patterned semiconductors as described in claim 1, characterized in that, The AgBiS2 solution is prepared as follows: Weigh out AgCl, BiCl3, and thiourea and dissolve them in N,N-dimethylformamide solution, stir to mix them evenly, wherein the concentration ratio of Ag:Bi:thiourea = 1:1:1.8; A SiO2 substrate with a patterned silver oxide seed layer is placed in a spin coater and rotated at a speed of no less than 2500 rpm for 60 seconds. During the rotation, a well-mixed AgBiS2 solution is added dropwise onto the SiO2 substrate to achieve spin coating. Then, it is heated in the range of 170-240 degrees Celsius for 5-10 minutes to achieve heating. The spin-coating-heating process was repeated three times to obtain micro-nano patterned AgBiS2 semiconductors on a SiO2 substrate.
7. A photoelectric imaging device fabricated using micro / nano patterning of semiconductors, characterized in that, include: SiO2 substrate (1), AgBiS2 linear array (4) and gold electrode (5) covering AgBiS2 linear array. The AgBiS2 linear array (4) is fabricated on the SiO2 substrate (1) using the semiconductor micro-nano patterning fabrication method as described in any one of claims 1 to 6. The linewidth of the AgBiS2 linear array (4) is no higher than 20 micrometers and the line spacing is no higher than 30 micrometers; Multiple gold electrodes (5) are arranged vertically above the AgBiS2 linear array (4), wherein the distance between adjacent gold electrodes (5) is no more than 100 micrometers, and the thickness of the gold electrodes (5) is between 50 and 100 nanometers.
8. The optoelectronic imaging device fabricated by micro-nano patterning of semiconductors as described in claim 7, characterized in that, The AgBiS2 linear array (4) has a line spacing of 20 micrometers and a line width of 10 micrometers.
9. The optoelectronic imaging device fabricated by micro-nano patterning of semiconductors as described in claim 7, characterized in that, The distance between each pair of gold electrodes is 50 micrometers, and each pair of gold electrodes (5) and the linear array between them constitute a device; each device contains 16 linear arrays.
10. The optoelectronic imaging device fabricated by micro-nano patterning of a semiconductor as described in claim 7, characterized in that, Gold electrodes (5) were deposited on a neatly arranged AgBiS2 linear array using a thermal evaporation method. The thickness of the gold electrodes (5) was 50 nanometers.