Aeolian sand pavement base material for preventing internal crack expansion and preparation method thereof
By presetting double spherical ceramic seam resistors in the base material of the wind-created sand pavement, using water glass and fiber to prevent crack expansion, the problem of road crack expansion in the existing technology is solved, and the service life of the road surface and the maintenance cost is reduced. Effect.
Patent Information
- Application Number
- CN202410030925.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-01-09
AI Technical Summary
The existing pavement restoration technology is mainly based on post-repair. It lacks preventive measures and it is difficult to effectively prevent the internal cracks in the wind-accumulated pavement, resulting in road damage and increased maintenance costs.
The seam resistor is preset in the base material of the wind-created sand pavement, and a double spherical ceramic structure is used to wrap water glass and fibers inside. The water glass and fibers are released through shear breaking to prevent cracks from spreading, which plays an anchoring role.
Effectively prevent the expansion of road cracks, extend the service life of the road, reduce maintenance costs, and improve construction efficiency and quality consistency through prefabricated block processes.
Smart Images

Figure CN117945726B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aeolian sand road surface base material preparation, in particular to aeolian sand road surface base material capable of preventing internal cracks from expanding and a preparation method thereof. Background Art
[0002] For the road surface, due to long-term vehicle traffic and the influence of the natural environment, various cracks and damage will appear, which will lead to an increase in the cost of road repair and maintenance, affecting the service life of the road and vehicle driving safety. Therefore, the research and development of anti-crack pavement materials has become one of the hot topics in the current road construction and transportation fields.
[0003] Existing road crack repairs mostly use a method of pouring slurry into the road cracks. For example, the patent with publication number CN115010454B discloses a concrete grouting material and its production process and a road surface repair process. In this scheme, the broken corners of the road surface are repaired by pouring an interface adhesive.
[0004] It can be seen that the existing pavement repair technologies are mainly based on post-repair, and there are few reports on methods that use aeolian sand and industrial solid waste as the main materials and pre-set joint blockers in the pavement base material. Summary of the invention
[0005] In order to achieve the above-mentioned purpose, the present invention provides a wind-blown sand pavement base material and a preparation method thereof that hinders the expansion of internal cracks. By pre-setting a crack blocker in the pavement base material, the expansion of pavement cracks can be effectively prevented, and small cracks can be prevented from developing into large cracks. The outer shell of the crack blocker is a double-spherical ceramic, which is wrapped with water glass inside, and a fiber outer layer is sintered at the junction of the double balls; when pavement cracks are generated, the shear force will cause the structural weak point of the crack blocker - the junction of the double balls to break, releasing the water glass inside. Under the joint obstruction of the water glass and the fibers between the balls, the pavement base material interface on both sides of the crack can be prevented from further separation, playing the role of anchoring the cracks. The scheme is shown below.
[0006] The present invention is a wind-blown sand pavement base material for preventing the expansion of internal cracks, wherein the components are calculated by mass ratio as follows:
[0007] Pretreated phosphogypsum: 10-20 parts, steel slag: 5-10 parts, slag: 5-10 parts, aeolian sand: 50-60 parts, silicate cement: 2-5 parts, joint blocker: 3-5 parts, PVA fiber: 0.3-2 parts, polycarboxylate water reducer 0.5-2 parts, water: 15-20 parts.
[0008] Description: Aeolian sand is a natural relic of weathering sand dunes, with relatively low acquisition costs and environmental impacts. Therefore, the use of aeolian sand to replace traditional sand and gravel aggregates to prepare pavement base materials has good economic and environmental benefits. In addition, the joint blocker is preset in the pavement base material in advance, and the joint blocker can be released continuously and slowly to ensure that the pavement can repair damaged parts over a longer period of time, extend the service life of the pavement, and greatly reduce subsequent maintenance costs.
[0009] The present invention also designs a method for preparing aeolian sand pavement base material that hinders the expansion of internal cracks. The finished product form of the pavement base material is a prefabricated block. The preparation steps of the prefabricated block are:
[0010] SA1. Pretreated phosphogypsum, steel slag, slag, aeolian sand, Portland cement, joint blocker, PVA fiber, polycarboxylate water reducer and water are mixed and uniformly mixed according to a proportion to obtain a first mixture;
[0011] SA2, placing the first mixed material in a mold and vibrating it, demoulding it after 20 to 24 hours to obtain a blank;
[0012] SA3. Take out the blanks after curing in the curing box for 28 days to obtain prefabricated blocks.
[0013] Description: By using prefabricated blocks, the pavement base material can be prepared in advance in the factory, reducing the complexity and construction period of on-site construction and improving construction efficiency. In addition, prefabricated blocks use fixed molds to ensure that the size, shape and quality of each block are consistent, reducing variability and quality problems during construction.
[0014] Furthermore, the preparation steps of the seam blocking agent are:
[0015] SB1, using A12O3 suspension as the base material, using DLP light-curing 3D printing technology to prepare A12O3 single-layer ring;
[0016] The parameters of DLP light-curing 3D printing technology are: UV light power is 1.05mW / cm 2 , exposure time is 30 to 40 seconds;
[0017] SB2, repeat the steps in SB1 to prepare A12O3 single-layer rings of various diameters, and add and bond the A12O3 single-layer rings of various diameters to obtain an A12O3 hollow double-ball blank; the sphere at one end of the A12O3 hollow double-ball blank is sealed, and the sphere at the other end is open;
[0018] The diameter of a single sphere of the A12O3 hollow double sphere blank is in the range of 10-12 mm, the diameter of the opening is in the range of 3-5 mm, and the diameter of the intersection of the two spheres is in the range of 5-6 mm;
[0019] SB3, coating 2-3 mm fiber mixture at the junction of double balls of A12O3 hollow double ball blank, and performing curing treatment;
[0020] According to the mass ratio, the composition of the fiber mixture is: A12O3 suspension: 30-35 parts, 50% by mass PVA fiber: 7-10 parts;
[0021] SB4, firing the A12O3 hollow double ball blank treated by SB3 under a temperature gradient to obtain an A12O3 hollow double ball finished product;
[0022] The temperature gradient is as follows: first, the temperature is increased from room temperature to 50°C at a rate of 4-5°C / min, and kept at this temperature for 7-10 minutes; then, the temperature is increased from 50°C to 200°C at a rate of 10-15°C / min, and kept at this temperature for 20-30 minutes; then, the temperature is increased from 200°C to 1000°C at a rate of 10-15°C / min, and kept at this temperature for 20-30 minutes; then, the temperature is increased from 1000°C to 1200°C at a rate of 2-3°C / min, and kept at this temperature for 1-1.5 hours; finally, the temperature is cooled to room temperature with the furnace;
[0023] SB5. Inject water glass into the opening at one end of the A12O3 hollow double ball product and seal it.
[0024] Description: The present invention adheres A12O3 single-layer circles of various diameters layer by layer in the shape of double balls by a layer-by-layer accumulation method, and then prepares a crack blocker by sintering. The outer shell of the crack blocker is double-spherical ceramic, the inside is wrapped with water glass, and a fiber outer layer is sintered at the junction of the double balls. When the shear force breaks the structural weak point of the crack blocker - the junction of the double balls, the water glass inside will be released, and the released water glass and the fibers between the balls can play a role in anchoring the interface cracks.
[0025] Further, the steps of preparing the A12O3 suspension in SB1 are:
[0026] SB1-1, disperse the pretreated Al2O3 powder in anhydrous ethanol, add OA, stir continuously at 80-85°C for 3-3.5h, and then dry at 80-90°C for 10-11h;
[0027] In SB1-1, according to the mass ratio, the amount of Al2O3 powder added is: 40-50 parts, the amount of OA added is: 3-5 parts, and the amount of anhydrous ethanol added is: 50-55 parts;
[0028] SB1-2, after drying, sieve the Al2O3 powder through an 80-mesh sieve, add it into HDDA, stir for 5 to 7 minutes, then add dichlorobis(dimethylphenylphosphonyl)zinc oxide, continue stirring for 30 to 40 minutes to obtain a mixture;
[0029] In SB1-2, the amount of Al2O3 powder added is 30-40 parts by weight, the amount of HDDA added is 20-30 parts, and the amount of dichlorobis(dimethylphenylphosphonyl)zinc oxide added is 2-3 parts by weight;
[0030] SB1-3, ball milling and defoaming the mixture in SB1-2 to obtain an A12O3 suspension;
[0031] Description: Adding substances such as dichlorobis(dimethylphenylphosphonyl)zinc oxide to the suspension can enhance the stability of the suspension, prevent particle sedimentation and precipitation, and maintain the long-term stability of the suspension; through ball milling and defoaming treatment, the particle size of Al2O3 particles in the suspension can be further controlled and refined to obtain the required particle size distribution and particle size, thereby improving the consistency and reliability of the particles.
[0032] Furthermore, the preparation steps of pre-treated Al2O3 powder in SB1-1 are:
[0033] SB1-1-1, place Al2O3 powder into 10% NaOH solution and stir continuously for 3 to 5 minutes;
[0034] SB1-1-2, wash the Al2O3 powder treated by SC1-1-1 with ethanol and deionized water respectively until the washing liquid is neutral;
[0035] SB1-1-3. Dry the Al2O3 powder treated by SB1-1-2 at 180-200°C for 10-11 hours to obtain pretreated Al2O3 powder.
[0036] Note: NaOH solution cleans and removes surface impurities, which can improve the purity and quality of Al2O3 powder. By using ethanol and deionized water to wash Al2O3 powder, the NaOH residue can be neutralized and the acidity and alkalinity of the powder can be adjusted to make it close to neutral, which helps to improve the operating results of subsequent steps and the stability of the product.
[0037] Further, the preparation steps of pre-treated phosphogypsum are:
[0038] SC1, firstly mix the acidic phosphogypsum and quicklime, then add water and mix evenly to obtain the second mixture;
[0039] According to the mass ratio, the amount of acidic phosphogypsum added is: 80-85 parts, the amount of quicklime added is: 1-1.5 parts, and the amount of water added is: 10-15 parts;
[0040] SC2. Place the second mixture in a sealed environment for 20 to 24 hours, and then dry it at 60 to 65°C for 20 to 30 minutes;
[0041] SC3. The dried second mixture is crushed through a sieve with a pore size of 1.18 mm to obtain pretreated phosphogypsum.
[0042] Note: The purpose of mixing acidic phosphogypsum with quicklime and water in the above method is to make alkaline adjustment. This reaction can neutralize the acidic properties of acidic phosphogypsum and convert it into a more stable compound to improve the durability of the base material.
[0043] Compared with the existing aeolian sand road base material, the present invention has the following beneficial effects:
[0044] (1) The present invention is a pavement base material that is designed to prevent the expansion of internal cracks. By pre-setting a crack blocking agent in the aeolian sand pavement base material, the expansion of pavement cracks can be effectively prevented, and small cracks can be prevented from developing into large cracks.
[0045] (2) The outer shell of the joint sealant designed in the present invention is a double-spherical ceramic, which is wrapped with water glass inside, and a fiber outer layer is sintered at the junction of the two balls. When pavement cracks are generated, the shear force will cause the structural weak point of the joint sealant - the junction of the two balls to break, releasing the water glass inside. Under the joint obstruction of the water glass and the fibers between the balls, the cement interfaces on both sides of the crack can be prevented from further separation, thereby playing the role of anchoring the crack. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a cross-sectional view of the seam barrier.
[0047] In the figure: 1-seal, 2-double ball blank, 3-fiber mixture, 4-glass water. DETAILED DESCRIPTION
[0048] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0049] Example 1: This example describes a wind-blown sand pavement base material that hinders the expansion of internal cracks and a preparation method thereof.
[0050] 1. The finished product form of the aeolian sand pavement base material is a prefabricated block, and the preparation steps of the prefabricated block are:
[0051] 1) pretreated phosphogypsum, steel slag, slag, aeolian sand, silicate cement, joint blocker, PVA fiber, polycarboxylate water reducer and water are mixed according to a proportion to obtain a first mixture;
[0052] 2) placing the first mixed material in a mold and vibrating it, and demolding it after 20 hours to obtain a blank;
[0053] 3) The blanks are cured in the curing box for 28 days and then taken out to obtain prefabricated blocks.
[0054] 2. The preparation steps of the joint blocking agent in the aeolian sand pavement base material are as follows:
[0055] 1) Place Al2O3 powder into a 10% NaOH solution and stir for 3 minutes;
[0056] 2) washing the Al2O3 powder with ethanol and deionized water respectively until the washing liquid is neutral;
[0057] 3) drying the Al2O3 powder at 180°C for 10 hours to obtain pretreated Al2O3 powder;
[0058] 4) Dispersing the pretreated Al2O3 powder in anhydrous ethanol, adding OA, stirring continuously at 80°C for 3 h, and then drying at 80°C for 10 h;
[0059] According to the mass ratio, the addition amount of Al2O3 powder is: 40 parts, the addition amount of OA is: 3 parts, and the addition amount of anhydrous ethanol is: 50 parts;
[0060] 5) Pass the dried Al2O3 powder through an 80-mesh sieve and add it to HDDA. After stirring for 5 minutes, add dichlorobis(dimethylphenylphosphonyl)zinc oxide and continue stirring for 30 minutes to obtain a mixture;
[0061] According to the mass ratio, the addition amount of Al2O3 powder is: 30 parts, the addition amount of HDDA is: 20 parts, and the addition amount of dichlorobis(dimethylphenylphosphonyl)zinc oxide is: 2 parts;
[0062] 6) ball milling and defoaming the mixture to obtain an Al2O3 suspension;
[0063] 7) Using A12O3 suspension as the base material, DLP light-curing 3D printing technology was used to prepare A12O3 single-layer ring;
[0064] The parameters of DLP light-curing 3D printing technology are: UV light power is 1.05mW / cm 2 , exposure time is 30s;
[0065] 8) Repeat the above steps to prepare A12O3 single-layer rings with various diameters, and add and bond the A12O3 single-layer rings with various diameters to obtain an A12O3 hollow double-ball blank; one end of the A12O3 hollow double-ball blank has a sealed sphere, and the other end has an open sphere;
[0066] The diameter of a single sphere of the A12O3 hollow double sphere blank is in the range of 10-12 mm, the diameter of the opening is 3 mm, and the diameter of the intersection of the double spheres is in the range of 5 mm;
[0067] 9) Coating 2mm fiber mixture at the intersection of the two balls of the A12O3 hollow double ball blank and performing curing treatment;
[0068] The composition of the fiber mixture according to the mass ratio is: A12O3 suspension: 30 parts, 50% by mass PVA fiber: 7 parts;
[0069] 10) firing the A12O3 hollow double ball blank under a temperature gradient to obtain an A12O3 hollow double ball finished product;
[0070] The temperature gradient is as follows: first, the temperature is increased from room temperature to 50°C at a rate of 4°C / min, and kept at this temperature for 7 minutes; then, the temperature is increased from 50°C to 200°C at a rate of 10°C / min, and kept at this temperature for 20 minutes; then, the temperature is increased from 200°C to 1000°C at a rate of 10°C / min, and kept at this temperature for 20 minutes; then, the temperature is increased from 1000°C to 1200°C at a rate of 2°C / min, and kept at this temperature for 1 hour; finally, the temperature is cooled to room temperature with the furnace;
[0071] 11) Inject water glass into the opening at one end of the finished A12O3 hollow double sphere and seal it.
[0072] 3. The preparation steps of pre-treated phosphogypsum are:
[0073] 1) firstly mixing acidic phosphogypsum with quicklime, and then adding water and mixing evenly to obtain a second mixture;
[0074] According to the mass ratio, the amount of acidic phosphogypsum added is 80 parts, the amount of quicklime added is 1 part, and the amount of water added is 10 parts;
[0075] 2) The second mixed material was placed in a sealed environment for 20 hours, and then dried at 60° C. for 20 minutes;
[0076] 3) The dried second mixture is crushed through a sieve with a pore size of 1.18 mm to obtain pretreated phosphogypsum.
[0077] 4. A wind-blown sand pavement base material for hindering the expansion of internal cracks prepared based on the methods in Sections 1 to 3, wherein the components are proportioned by mass as follows: pretreated phosphogypsum: 10 parts, steel slag: 5 parts, slag: 5 parts, wind-blown sand: 50 parts, silicate cement: 2 parts, joint blocker: 3 parts, PVA fiber: 0.3 parts, polycarboxylate water reducer 0.5 parts, and water: 15 parts.
[0078] Example 2: This example describes a wind-blown sand pavement base material that hinders the expansion of internal cracks and a preparation method thereof.
[0079] 1. The finished product form of the aeolian sand pavement base material is a prefabricated block, and the preparation steps of the prefabricated block are:
[0080] 1) pretreated phosphogypsum, steel slag, slag, aeolian sand, silicate cement, joint blocker, PVA fiber, polycarboxylate water reducer and water are mixed according to a proportion to obtain a first mixture;
[0081] 2) placing the first mixed material in a mold and vibrating it, and demolding it after 24 hours to obtain a blank;
[0082] 3) The blanks are cured in the curing box for 28 days and then taken out to obtain prefabricated blocks.
[0083] 2. The preparation steps of the joint blocking agent in the aeolian sand pavement base material are as follows:
[0084] 1) Place Al2O3 powder into 10% NaOH solution and stir for 5 minutes;
[0085] 2) washing the Al2O3 powder with ethanol and deionized water respectively until the washing liquid is neutral;
[0086] 3) drying the Al2O3 powder at 200°C for 11 hours to obtain pretreated Al2O3 powder;
[0087] 4) Disperse the pretreated Al2O3 powder in anhydrous ethanol, add OA, stir continuously at 85°C for 3.5h, and then dry at 90°C for 11h;
[0088] According to the mass ratio, the addition amount of Al2O3 powder is: 50 parts, the addition amount of OA is: 5 parts, and the addition amount of anhydrous ethanol is: 55 parts;
[0089] 5) The dried Al2O3 powder was sieved through an 80-mesh sieve and added to HDDA. After stirring for 7 minutes, dichlorobis(dimethylphenylphosphonyl)zinc oxide was added and the mixture was stirred for 40 minutes to obtain a mixture.
[0090] According to the mass ratio, the addition amount of Al2O3 powder is: 40 parts, the addition amount of HDDA is: 30 parts, and the addition amount of dichlorobis(dimethylphenylphosphonyl)zinc oxide is: 3 parts;
[0091] 6) ball milling and defoaming the mixture to obtain an Al2O3 suspension;
[0092] 7) Using A12O3 suspension as the base material, DLP light-curing 3D printing technology was used to prepare A12O3 single-layer ring;
[0093] The parameters of DLP light-curing 3D printing technology are: UV light power is 1.05mW / cm 2 , the exposure time is 40s;
[0094] 8) Repeat the above steps to prepare A12O3 single-layer rings with various diameters, and add and bond the A12O3 single-layer rings with various diameters to obtain an A12O3 hollow double-ball blank; one end of the A12O3 hollow double-ball blank has a sealed sphere, and the other end has an open sphere;
[0095] The diameter of a single sphere of the A12O3 hollow double sphere billet is in the range of 12 mm, the diameter of the opening is 5 mm, and the diameter of the intersection of the two spheres is in the range of 6 mm;
[0096] 9) Coating 3mm fiber mixture at the intersection of the two balls of the A12O3 hollow double ball blank and performing curing treatment;
[0097] The composition of the fiber mixture according to the mass ratio is: A12O3 suspension: 35 parts, 50% by mass PVA fiber: 10 parts;
[0098] 10) firing the A12O3 hollow double ball blank under a temperature gradient to obtain an A12O3 hollow double ball finished product;
[0099] The temperature gradient is as follows: first, the temperature is increased from room temperature to 50°C at a rate of 5°C / min, and kept at this temperature for 10 minutes; then, the temperature is increased from 50°C to 200°C at a rate of 15°C / min, and kept at this temperature for 30 minutes; then, the temperature is increased from 200°C to 1000°C at a rate of 15°C / min, and kept at this temperature for 30 minutes; then, the temperature is increased from 1000°C to 1200°C at a rate of 3°C / min, and kept at this temperature for 1.5 hours; finally, the temperature is cooled to room temperature with the furnace;
[0100] 11) Inject water glass into the opening at one end of the finished A12O3 hollow double sphere and seal it.
[0101] 3. The preparation steps of pre-treated phosphogypsum are:
[0102] 1) firstly mixing acidic phosphogypsum with quicklime, and then adding water and mixing evenly to obtain a second mixture;
[0103] According to the mass ratio, the amount of acidic phosphogypsum added is 85 parts, the amount of quicklime added is 1.5 parts, and the amount of water added is 15 parts;
[0104] 2) The second mixed material was placed in a sealed environment for 24 hours, and then dried at 65° C. for 30 minutes;
[0105] 3) The dried second mixture is crushed through a sieve with a pore size of 1.18 mm to obtain pretreated phosphogypsum.
[0106] 4. A wind-blown sand pavement base material for hindering the expansion of internal cracks prepared based on the methods in Sections 1 to 3, wherein the components are proportioned by mass as follows: pretreated phosphogypsum: 20 parts, steel slag: 10 parts, slag: 10 parts, wind-blown sand: 60 parts, silicate cement: 5 parts, joint blocker: 5 parts, PVA fiber: 2 parts, polycarboxylic acid water reducer 2 parts, and water: 20 parts.
[0107] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention.
[0108] 1. Experimental design: In order to illustrate the flexural properties of the aeolian sand pavement base material prepared by the present invention, the following experimental groups were designed:
[0109] For the convenience of the experiment, a test sample of aeolian sand pavement base material was prepared by the method in Example 1, and the mold size was 10*5*2cm; the components in the test sample were proportioned by mass as follows: pretreated phosphogypsum: 10 parts, steel slag: 5 parts, slag: 5 parts, aeolian sand: 50 parts, silicate cement: 2 parts, joint blocker: 3 parts, PVA fiber: 0.3 parts, polycarboxylate water reducer 0.5 parts, and water: 15 parts.
[0110] The flexural strength of the test sample was tested on the 30th day after molding. The testing method was as follows: fix one end of the long side of the test sample, apply static pressure on the other side until cracks appear on the test sample, and then test the flexural strength of the sample again after standing for 1 day.
[0111] Blank group: No sealant was added to the test sample;
[0112] Control group 1: 1 portion of seam blocker was added to the test sample;
[0113] Control group 2: 2 parts of seam blocker were added to the test sample;
[0114] Control group 3: 3 parts of seam blocker were added to the test sample;
[0115] Control group 4: 4 parts of seam blocker were added to the test sample;
[0116] Control group 5: 5 parts of seam blocker were added to the test sample;
[0117] Control group 6: 6 parts of seam blocker were added to the test sample;
[0118] Control group 7: 7 parts of seam sealant were added to the test sample.
[0119] 2. Related performance experiments: The actual performance of the present invention under different experimental conditions is compared, and the specific data are shown in Table 1.
[0120] Table 1 Experimental data
[0121]
[0122] First of all, it can be seen from the data in Table 1 that as the amount of seam barrier added gradually increases, the initial flexural strength of the tested sample gradually decreases. This is because the structure of the seam barrier itself will cause a "bridging" phenomenon in the ingredient components. The increase in the addition of seam barrier will lead to a decrease in the density of the original material, thereby reducing the overall strength of the sample.
[0123] In the blank group, cracks occurred in the samples but they could not be healed subsequently, so no data was recorded.
[0124] Comparing the data of control groups 1 to 7, it can be seen that with the increase in the amount of crack blocker added, the strength recovery amplitude of the sample one day after the crack is generated first shows an upward trend, and then a downward trend, and the turning point is control group 6; it is speculated that the reason for the above phenomenon is: excessive addition of crack blocker destroys the bonding strength between other components, thereby reducing the overall crack resistance of the material. Therefore, in practical applications, the appropriate component ratio should be selected according to needs.
Claims
1. A method for preparing a wind-blown sand pavement base material that hinders the expansion of internal cracks, wherein the components in the pavement base material are as follows by mass ratio: Pre-treated phosphogypsum: 10-20 parts, steel slag: 5-10 parts, slag: 5-10 parts, aeolian sand: 50-60 parts, silicate cement: 2-5 parts, joint blocker: 3-5 parts, PVA fiber: 0.3-2 parts, polycarboxylate water reducer 0.5-2 parts, water: 15-20 parts; It is characterized in that The preparation steps of the seam blocking agent are as follows: SB1, using A12O3 suspension as the base material, using DLP light-curing 3D printing technology to prepare A12O3 single-layer ring; The parameters of DLP light-curing 3D printing technology are: UV light power is 1.05mW / cm 2 , exposure time is 30 to 40 seconds; SB2, repeat the steps in SB1 to prepare A12O3 single-layer rings of various diameters, and add and bond the A12O3 single-layer rings of various diameters to obtain an A12O3 hollow double-ball blank; the A12O3 hollow double-ball blank has a sealed sphere at one end and an open sphere at the other end; The diameter of a single sphere of the A12O3 hollow double sphere blank is in the range of 10 to 12 mm, the diameter of the opening is in the range of 3 to 5 mm, and the diameter of the intersection of the double spheres is in the range of 5 to 6 mm; SB3, coating 2-3 mm fiber mixture at the junction of double balls of A12O3 hollow double ball blank, and performing curing treatment; According to the mass ratio, the fiber mixture is composed of: A12O3 suspension: 30-35 parts, 50% by mass of PVA fiber: 7-10 parts; SB4, firing the A12O3 hollow double ball blank treated by SB3 under a temperature gradient to obtain an A12O3 hollow double ball finished product; The temperature gradient is as follows: first, the temperature is increased from room temperature to 50°C at a rate of 4-5°C / min, and kept at this temperature for 7-10 minutes; then, the temperature is increased from 50°C to 200°C at a rate of 10-15°C / min, and kept at this temperature for 20-30 minutes; then, the temperature is increased from 200°C to 1000°C at a rate of 10-15°C / min, and kept at this temperature for 20-30 minutes; then, the temperature is increased from 1000°C to 1200°C at a rate of 2-3°C / min, and kept at this temperature for 1-1.5 hours; finally, the temperature is cooled to room temperature with the furnace; SB5. Inject water glass into the opening at one end of the A12O3 hollow double ball product and seal it.
2. The method for preparing a wind-blown sand pavement base material for hindering the expansion of internal cracks according to claim 1, characterized in that: The steps of preparing the Al2O3 suspension in the SB1 are: SB1-1, disperse the pretreated Al2O3 powder in anhydrous ethanol, add OA, stir continuously at 80-85°C for 3-3.5h, and then dry at 80-90°C for 10-11h; In SB1-1, according to the mass ratio, the amount of Al2O3 powder added is: 40-50 parts, the amount of OA added is: 3-5 parts, and the amount of anhydrous ethanol added is: 50-55 parts; SB1-2, after drying, sieve the Al2O3 powder through an 80-mesh sieve, add it into HDDA, stir for 5 to 7 minutes, then add dichlorobis(dimethylphenylphosphonyl)zinc oxide, continue stirring for 30 to 40 minutes to obtain a mixture; In SB1-2, the amount of Al2O3 powder added is 30-40 parts by weight, the amount of HDDA added is 20-30 parts, and the amount of dichlorobis(dimethylphenylphosphonyl)zinc oxide added is 2-3 parts by weight; SB1-3. The mixture described in SB1-2 is ball-milled and defoamed to obtain an A12O3 suspension.
3. The method for preparing a wind-blown sand pavement base material for hindering the expansion of internal cracks as claimed in claim 2, characterized in that: The preparation steps of the pre-treated Al2O3 powder in SB1-1 are as follows: SB1-1-1, place Al2O3 powder into 10% NaOH solution and stir continuously for 3 to 5 minutes; SB1-1-2, wash the Al2O3 powder treated by SC1-1-1 with ethanol and deionized water respectively until the washing liquid is neutral; SB1-1-3. Dry the Al2O3 powder treated by SB1-1-2 at 180-200°C for 10-11 hours to obtain pretreated Al2O3 powder.
4. The method for preparing a wind-blown sand pavement base material for hindering the expansion of internal cracks according to claim 1, characterized in that: The finished product form of the pavement base material is a prefabricated block, and the preparation steps of the prefabricated block are: SA1. Mix the pretreated phosphogypsum, steel slag, slag, aeolian sand, Portland cement, joint blocker, PVA fiber, polycarboxylate water reducer and water according to a proportion to obtain a first mixture; SA2, placing the first mixture in a mold and vibrating it, demoulding it after 20 to 24 hours to obtain a blank; SA3. Curing the blank in a curing box for 28 days, and then taking it out to obtain a prefabricated block.
5. The method for preparing a wind-blown sand pavement base material for preventing the expansion of internal cracks according to claim 1, characterized in that: The preparation steps of the pretreated phosphogypsum are: SC1, firstly mix the acidic phosphogypsum and quicklime, then add water and mix evenly to obtain the second mixture; According to the mass ratio, the amount of acidic phosphogypsum added is: 80-85 parts, the amount of quicklime added is: 1-1.5 parts, and the amount of water added is: 10-15 parts; SC2, leaving the second mixture in a sealed environment for 20 to 24 hours, and then drying at 60 to 65° C. for 20 to 30 minutes; SC3. The dried second mixture is crushed through a sieve with a pore size of 1.18 mm to obtain pretreated phosphogypsum.