Nano-matt paint for wooden floor and preparation method thereof

By using end-hydroxypropyl polydimethylsiloxane and epoxy resin in paint for wood flooring, a matting resin with crosslinking structure and high silicone oxygen bond is generated, combining nano-silica and thickener Raw materials such as chitosan solve the problems of existing low-gloss water-based polyurethane paint in terms of stability and scratch resistance after the introduction of matting agent, and achieve excellent matting, water resistance and self-repair performance.

CN117965088BActive Publication Date: 2024-11-29GUANGDONG NATURE HOME FURNISHING TECH RES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410188892.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-20
Publication Date
2024-11-29
Estimated Expiration
2044-02-20

AI Technical Summary

Technical Problem

The existing low-gloss water-based polyurethane paints are easily reduced by the stability and scratch resistance of the emulsion after the introduction of the matting agent, and the new single-component WPU without matting agent is poor in water resistance, thermal stability and mechanical properties.

Method used

By preparing a nanomatte paint for wooden flooring, copolymerizing with end-hydroxypropyl polydimethylsiloxane with epoxy resin, it generates a mattressing resin with crosslinking structure and high silicon oxygen bonds, and combines nanosilicon dioxide. , thickener and chitosan to form a paint film with excellent extinction, water resistance and self-healing properties.

Benefits of technology

It realizes excellent extinction of nanomatte paint for wooden floors, improves the water resistance and mechanical properties of the paint film, and gives it self-healing ability, enhancing the stability and scratch resistance of the paint film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004707075010000031
    Figure BDA0004707075010000031
  • Figure BDA0004707075010000032
    Figure BDA0004707075010000032
  • Figure BDA0004707075010000041
    Figure BDA0004707075010000041
Patent Text Reader

Abstract

The invention discloses a nano-matt paint for wood flooring and a preparation method thereof, comprising the following raw materials in parts by weight: 60-70 parts of matt resin, 5-7 parts of thickener, 3-5 parts of hand wax powder, 3-5 parts of nano-silicon dioxide dispersion, 1-3 parts of water-based color essence, 1-2 parts of wetting agent, 0.5-1 parts of defoamer, 1-1.5 parts of dispersant and 20-30 parts of deionized water. The matt resin obtained by using epoxy resin modified terminal hydroxypropyl polydimethylsiloxane to participate in copolymerization of aqueous polyurethane enhances the water resistance and mattness of matt paint film; the introduction of chitosan makes the paint film have good self-repairing properties; the introduction of acrylate groups makes matt paint have UV curable properties. The thickener molecule has a benzophenone structure, which makes it thicken in the matt paint and play a photoinitiating role at the same time. After UV curing, the thickener and the matt resin are chemically connected, which can effectively reduce the migration and penetration of the thickener in the cured coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of matte paint, and in particular to a nano matte paint for wooden floors and a preparation method thereof. Background Art

[0002] Waterborne polyurethane (WPU) has the advantages of high film strength, good wear resistance, non-toxicity and green environmental protection. With the continuous improvement of people's aesthetic concepts, low-gloss WPU has attracted much attention. Traditional low-gloss WPU is made by adding a matting agent to the polyurethane (PU) dispersion. The matting agent will float on the surface of the film during the drying process of the film and make the microstructure of the film surface uneven, thereby achieving the purpose of matting. However, the introduction of the matting agent can easily reduce the stability and scratch resistance of the emulsion. Previous studies have found a new type of single-component WPU with matting properties without adding a matting agent, but its water resistance, thermal stability and mechanical properties are poor. In order to improve the comprehensive performance of WPU matting resin and expand its application range, it must be modified.

[0003] From preparation to the final decorative paint film, water-based paint needs to go through four processes: preparation, storage, painting, and leveling. Different stages require different viscosities of the paint system. For example, during the production process, the paint is required to have a certain viscosity to prevent liquid splashing due to high-speed stirring and shearing during the paint preparation process, and at the same time promote a more complete dispersion of various additives and fillers; during storage, the paint is required to maintain a high viscosity under low shear conditions to prevent the powder in the paint from settling downward due to gravity and causing stratification, thereby improving the stability of the paint system; during the painting stage, the paint is required to have a certain thixotropy, so that the paint maintains a certain low viscosity under the action of shear forces such as spraying, ensuring smooth painting and good leveling of the coating on the substrate; after the coating is leveled, the paint is required to quickly return to a higher viscosity to prevent the coating from sagging and no droplets splashing when rolling. With the increasing diversification of current paint viscosity requirements, existing thickeners are far from meeting the requirements. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a nano matte paint for wooden floor and a preparation method thereof.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A nano matte paint for wood flooring comprises the following raw materials in parts by weight: 60-70 parts of matting resin, 5-7 parts of thickener, 3-5 parts of hand wax powder, 3-5 parts of nano silicon dioxide dispersion, 1-3 parts of water-based color essence, 1-2 parts of wetting agent, 0.5-1 parts of defoaming agent, 1-1.5 parts of dispersant and 20-30 parts of deionized water.

[0007] The hand wax powder is polytetrafluoroethylene wax powder.

[0008] The wetting agent is polyether silicone oil.

[0009] The defoaming agent is polydimethylsiloxane.

[0010] The dispersant is an ammonium polyacrylate dispersant.

[0011] The matt resin is prepared by the following steps:

[0012] Step A1: Dry the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol under vacuum at 100° C. for 1 h and set aside. Add terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol to a flask equipped with a thermometer, a stirrer and a condenser, heat to 90°C, add toluene diisocyanate and a catalyst dibutyltin diisocyanate under stirring, react at a constant temperature for 4 hours, cool to 50°C, add 2,2-dihydroxymethylpropionic acid and tetrahydrofuran to the flask, heat to 70°C, react at a constant temperature for 2 hours, and cool to room temperature to obtain intermediate 1, terminal hydroxypropyl polydimethylsiloxane, polyethylene glycol, toluene diisocyanate, dibutyltin diisocyanate, 2,2-dihydroxymethylpropionic acid and tetrahydrofuran in a ratio of 0.3 mol: 0.1 mol: 0.1-0.12 mol: 0.0015 mol: 0.002-0.003 mol: 250-300 mL;

[0013] During the reaction, the hydroxyl groups of the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol react with the isocyanate group of toluene diisocyanate respectively, and 2,2-dihydroxymethyl propionic acid reacts with the isocyanate group as a hydrophilic chain extender to generate intermediate 1. The structure of intermediate 1 is shown below:

[0014]

[0015] Step A2: under nitrogen protection, add bisphenol A epoxy resin E-12 to toluene, start stirring, slowly add intermediate 1 thereto, continue to react at 70-80°C for 1-1.5h, wait until the system temperature drops to room temperature to obtain a reaction liquid, pour the reaction liquid into an emulsification barrel, add triethylamine and deionized water, and prepare intermediate 2 under high-speed stirring and shearing, the dosage ratio of bisphenol A epoxy resin E-12, toluene, intermediate 1, triethylamine and deionized water is: 0.1-0.13g:70mL:2-2.5g:0.08g:60mL;

[0016] During the reaction, the epoxy group and secondary hydroxyl group in the bisphenol A epoxy resin E-12 react with the isocyanate group in the intermediate 1 to produce a cross-linked structure. The triethylamine neutralizes the carboxyl group introduced by the hydrophilic chain extender 2,2-dimethylol propionic acid to obtain the intermediate 2. The structure of the intermediate 2 is shown below:

[0017]

[0018] Step A3: adding chitosan and diethylamine to the intermediate 2, stirring and reacting at a speed of 600 r / min and 60° C. for 5-6 hours, cooling to 40° C., and then adding pentaerythritol triacrylate, stirring and reacting for 3-4 hours to obtain a matte resin, wherein the amount ratio of the intermediate 2, chitosan, diethylamine and pentaerythritol triacrylate is 2.6-3.0 g: 0.2-0.3 g: 0.5-0.6 g: 0.33-0.40 g;

[0019] During the reaction, the hydroxyl group and amino group of chitosan react with the isocyanate group of intermediate 2 respectively, the amino group of diethylamine reacts with the isocyanate group of intermediate 2, and the remaining unreacted terminal isocyanate group reacts with pentaerythritol triacrylate to obtain a matting resin. The terminal hydroxypropyl polydimethylsiloxane contains a silicon-oxygen bond, which gives the molecular chain excellent flexibility, and the silicon-oxygen bond has high bond energy and good heat resistance. It is introduced into the system by copolymerization to prepare an emulsion. After film formation, the silicone polymer migrates to the surface to produce a microscopically rough surface, thereby enhancing diffuse reflection and achieving a matte effect; the epoxy group and secondary hydroxyl group in the introduced epoxy resin are copolymerized with the water-based polyurethane to produce a cross-linked structure, and the branching point is introduced into the main chain of the polyurethane. The rigid structure of the benzene ring introduced together improves the water resistance of the matte resin. After emulsification with water, a regular microsphere-type stable emulsion is formed. After the emulsion is dried and formed into a film, the microspheres with larger particle size are easily visible on the surface of the coating, resulting in a microscopically rough structure, and thus having excellent matte properties; the introduction of chitosan as a chain extender gives the matte resin good self-healing properties; the introduction of acrylate groups makes the matte resin UV-curable.

[0020] The thickener is prepared by the following steps:

[0021] Step B1: Add 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF into a three-necked flask, and react with stirring at 80° C. for 12 h under nitrogen protection, extract with dichloromethane, dry, and rotary evaporate to obtain intermediate a, wherein the amount ratio of 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF is 0.15 mol: 0.18 mol: 0.30 mol: 50-60 mL;

[0022] During the reaction, 2-hydroxy-4-n-octyloxybenzophenone and 11-bromo-undecanol undergo etherification reaction to generate intermediate a. The structure of intermediate a is shown below:

[0023]

[0024] Step B2: Add polyethylene glycol and toluene to a flask, heat to 130°C under nitrogen protection, distill for 1.5-2h, cool to 60-70°C, add dibutyltin dilaurate and isophorone diisocyanate to the flask, stir and react at 80°C for 3.5-4h, then add intermediate a to the flask, stir and react at 85°C for 16h to obtain a mixed solution, cool the mixed solution to room temperature, recrystallize with ether, filter, add dichloromethane to the filter cake, and recrystallize with ether to obtain a thickener, wherein the amount ratio of polyethylene glycol, toluene, dibutyltin dilaurate, isophorone diisocyanate and intermediate a is 0.25mmol:150mL:0.01g:2.5mmol:5mmol;

[0025] During the reaction, the terminal hydroxyl group of polyethylene glycol reacts with the isocyanate group of isophorone diisocyanate, and then the remaining terminal isocyanate group reacts with the hydroxyl group of intermediate a to obtain a thickener. The benzophenone structure is introduced into the thickener molecule through the reaction. The introduced benzophenone structure enables the thickener to play a photoinitiating role while playing a thickening role. After UV curing, the thickener can be chemically connected with the UV-curable matting resin through a hydrogen abstraction coupling reaction.

[0026] Beneficial effects of the present invention: the nano matt paint for wood flooring prepared by the present invention includes raw materials such as matt resin, hand wax powder, nano silicon dioxide dispersion, thickener, water-based color essence, wetting agent, defoamer, dispersant and deionized water. The matt resin used is obtained by modifying the water-based polyurethane in which terminal hydroxypropyl polydimethylsiloxane is copolymerized with epoxy resin. Terminal hydroxypropyl polydimethylsiloxane contains silicon-oxygen bonds with high bond energy and good heat resistance. It is introduced into the system by copolymerization to prepare an emulsion. After film formation, the organic silicon polymer migrates to the surface of the matt paint film to produce a microscopically rough surface, thereby enhancing diffuse reflection to achieve the effect of matt. The epoxy groups and secondary hydroxyls in the introduced epoxy resin are copolymerized with the water-based polyurethane to produce a cross-linked structure, and the branching points are introduced into the main chain of the polyurethane. The rigid structure of the benzene ring introduced together improves the water resistance of the matt resin. After emulsification with water, a regular microsphere-type stable emulsion is formed. The emulsion dries After drying and film formation, microspheres with larger particle size are easily visible on the surface of the matte paint film, resulting in a microscopic rough structure, thus having excellent matting properties; and the introduced epoxy resin has the characteristics of high strength, high hardness and excellent anti-corrosion performance, which can improve the mechanical properties of the matte paint film; the introduction of chitosan gives the matte resin good self-healing properties, so that scratches on the surface of the matte paint film can recover by themselves, and its repair properties come from the exchange reaction between the hydroxyl group of chitosan and the polyurethane group in the matte paint film at high temperature; the introduction of acrylate groups makes the matte paint have UV-curable properties.

[0027] The thickener used is a reactive polyurethane thickener. By synthesizing benzophenone derivatives as end-capping agents for polyurethane, a benzophenone structure is introduced into the thickener structure, so that the thickener can play a thickening role in the matte paint while also playing a photoinitiating role. After UV curing, the thickener can be chemically connected with the UV-curable matting resin through a hydrogen abstraction coupling reaction, which can effectively reduce the migration and penetration of the thickener in the cured coating of the matte paint. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A matte resin is prepared by the following steps:

[0031] Step A1: Dry the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol at 100°C in vacuum for 1h and set aside. Add terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol to a flask equipped with a thermometer, a stirrer and a condenser, heat to 90°C, add toluene diisocyanate and catalyst dibutyltin diisocyanate under stirring, react at constant temperature for 4h, cool to 50°C, add 2,2-dihydroxymethylpropionic acid and tetrahydrofuran to the flask, heat to 70°C and react at constant temperature for 2h, cool to room temperature, and obtain intermediate 1, terminal hydroxypropyl polydimethylsiloxane, polyethylene glycol, toluene diisocyanate, dibutyltin diisocyanate, 2,2-dihydroxymethylpropionic acid and tetrahydrofuran in a ratio of 0.3mol:0.1mol:0.1mol:0.0015mol:0.002mol:250mL;

[0032] Step A2: under nitrogen protection, bisphenol A epoxy resin E-12 was added to toluene, stirring was started, intermediate 1 was slowly added thereto, and the reaction was continued at 70°C for 1 hour. When the system temperature dropped to room temperature, a reaction liquid was obtained, and the reaction liquid was poured into an emulsification barrel, triethylamine and deionized water were added, and intermediate 2 was obtained under high-speed stirring and shearing. The dosage ratio of bisphenol A epoxy resin E-12, toluene, intermediate 1, triethylamine and deionized water was: 0.1g:70mL:2g:0.08g:60mL;

[0033] Step A3: chitosan and diethylamine were added to the intermediate 2, and the mixture was stirred at 600 r / min and 60° C. for 5 h. The temperature was lowered to 40° C., and pentaerythritol triacrylate was added, and the mixture was stirred for 3 h to obtain a matte resin. The amount ratio of the intermediate 2, chitosan, diethylamine and pentaerythritol triacrylate was 2.6 g: 0.2 g: 0.5 g: 0.33 g.

[0034] Example 2

[0035] A matte resin is prepared by the following steps:

[0036] Step A1: Dry the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol at 100°C in vacuum for 1 hour and set aside. Add the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol to a flask equipped with a thermometer, a stirrer and a condenser, heat to 90°C, add toluene diisocyanate and the catalyst dibutyltin diisocyanate under stirring, react at constant temperature for 4 hours, cool to 50°C, add 2,2-dihydroxymethylpropionic acid and tetrahydrofuran to the flask, heat to 70°C and react at constant temperature for 2 hours, cool to room temperature, and obtain intermediate 1, the amount ratio of terminal hydroxypropyl polydimethylsiloxane, polyethylene glycol, toluene diisocyanate, dibutyltin diisocyanate, 2,2-dihydroxymethylpropionic acid and tetrahydrofuran is 0.3 mol: 0.1 mol: 0.11 mol: 0.0015 mol: 0.0025 mol: 280 mL;

[0037] Step A2: under nitrogen protection, bisphenol A epoxy resin E-12 was added to toluene, stirring was started, intermediate 1 was slowly added thereto, and the reaction was continued at 75° C. for 1.2 h. When the system temperature dropped to room temperature, a reaction solution was obtained. The reaction solution was poured into an emulsification barrel, triethylamine and deionized water were added, and intermediate 2 was obtained under high-speed stirring and shearing. The dosage ratio of bisphenol A epoxy resin E-12, toluene, intermediate 1, triethylamine and deionized water was: 0.12 g: 70 mL: 2.2 g: 0.08 g: 60 mL;

[0038] Step A3: chitosan and diethylamine were added to intermediate 2, and the mixture was stirred at 600 r / min and 60° C. for 5.5 h. The temperature was lowered to 40° C., and pentaerythritol triacrylate was added, and the mixture was stirred for 3.5 h to obtain a matte resin. The amount ratio of intermediate 2, chitosan, diethylamine and pentaerythritol triacrylate was 2.8 g: 0.25 g: 0.55 g: 0.37 g.

[0039] Example 3

[0040] A matte resin is prepared by the following steps:

[0041] Step A1: Dry the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol at 100°C in vacuum for 1 hour and set aside. Add the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol to a flask equipped with a thermometer, a stirrer and a condenser, heat to 90°C, add toluene diisocyanate and a catalyst dibutyltin diisocyanate under stirring, react at a constant temperature for 4 hours, cool to 50°C, add 2,2-dihydroxymethylpropionic acid and tetrahydrofuran to the flask, heat to 70°C, react at a constant temperature for 2 hours, cool to room temperature, and obtain intermediate 1, the amount ratio of terminal hydroxypropyl polydimethylsiloxane, polyethylene glycol, toluene diisocyanate, dibutyltin diisocyanate, 2,2-dihydroxymethylpropionic acid and tetrahydrofuran is 0.3 mol: 0.1 mol: 0.12 mol: 0.0015 mol: 0.003 mol: 300 mL;

[0042] Step A2: under nitrogen protection, bisphenol A epoxy resin E-12 was added to toluene, stirring was started, intermediate 1 was slowly added thereto, and the reaction was continued at 80°C for 1.5 hours. When the system temperature dropped to room temperature, a reaction liquid was obtained, and the reaction liquid was poured into an emulsification barrel, triethylamine and deionized water were added, and intermediate 2 was obtained under high-speed stirring and shearing. The dosage ratio of bisphenol A epoxy resin E-12, toluene, intermediate 1, triethylamine and deionized water was: 0.13 g: 70 mL: 2.5 g: 0.08 g: 60 mL;

[0043] Step A3: chitosan and diethylamine were added to the intermediate 2, and the mixture was stirred at 600 r / min and 60°C for 6 h. The temperature was lowered to 40°C, and pentaerythritol triacrylate was added, and the mixture was stirred for 4 h to obtain a matte resin. The amount ratio of the intermediate 2, chitosan, diethylamine and pentaerythritol triacrylate was 3.0 g: 0.3 g: 0.6 g: 0.40 g.

[0044] Example 4

[0045] A thickener is prepared by the following steps:

[0046] Step B1: Add 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF into a three-necked flask, and react with stirring at 80° C. for 12 h under nitrogen protection, extract with dichloromethane, dry, and rotary evaporate to obtain intermediate a, wherein the amount ratio of 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF is 0.15 mol: 0.18 mol: 0.30 mol: 50 mL;

[0047] Step B2: Add polyethylene glycol and toluene to a flask, heat to 130°C under nitrogen protection, distill for 1.5 hours, cool to 60°C, add dibutyltin dilaurate and isophorone diisocyanate to the flask, stir and react at 80°C for 3.5 hours, then add intermediate a to the above flask, stir and react at 85°C for 16 hours to obtain a mixed solution, cool the mixed solution to room temperature, recrystallize with ether, filter, add dichloromethane to the filter cake, and recrystallize with ether to obtain a thickener. The amount ratio of polyethylene glycol, toluene, dibutyltin dilaurate, isophorone diisocyanate and intermediate a is 0.25mmol:150mL:0.01g:2.5mmol:5mmol.

[0048] Example 5

[0049] A thickener is prepared by the following steps:

[0050] Step B1: Add 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF into a three-necked flask, and react with stirring at 80° C. for 12 h under nitrogen protection, extract with dichloromethane, dry, and rotary evaporate to obtain intermediate a, wherein the amount ratio of 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF is 0.15 mol: 0.18 mol: 0.30 mol: 55 mL;

[0051] Step B2: Add polyethylene glycol and toluene to a flask, heat to 130°C under nitrogen protection, distill for 1.8 hours, cool to 65°C, add dibutyltin dilaurate and isophorone diisocyanate to the flask, stir and react at 80°C for 3.7 hours, then add intermediate a to the flask, stir and react at 85°C for 16 hours to obtain a mixed solution, cool the mixed solution to room temperature, recrystallize with ether, filter, add dichloromethane to the filter cake, and recrystallize with ether to obtain a thickener. The amount ratio of polyethylene glycol, toluene, dibutyltin dilaurate, isophorone diisocyanate and intermediate a is 0.25mmol:150mL:0.01g:2.5mmol:5mmol.

[0052] Example 6

[0053] A thickener is prepared by the following steps:

[0054] Step B1: Add 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF into a three-necked flask, and react with stirring at 80° C. for 12 h under nitrogen protection, extract with dichloromethane, dry, and rotary evaporate to obtain intermediate a, wherein the amount ratio of 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF is 0.15 mol: 0.18 mol: 0.30 mol: 60 mL;

[0055] Step B2: Add polyethylene glycol and toluene to a flask, heat to 130°C under nitrogen protection, distill for 2 hours, cool to 70°C, add dibutyltin dilaurate and isophorone diisocyanate to the flask, stir and react at 80°C for 4 hours, then add intermediate a to the flask, stir and react at 85°C for 16 hours to obtain a mixed solution, cool the mixed solution to room temperature, recrystallize with ether, filter, add dichloromethane to the filter cake, and recrystallize with ether to obtain a thickener. The amount ratio of polyethylene glycol, toluene, dibutyltin dilaurate, isophorone diisocyanate and intermediate a is 0.25mmol:150mL:0.01g:2.5mmol:5mmol.

[0056] Example 7

[0057] A nano matte paint for wood flooring includes the following raw materials by weight: 60 parts of matting resin, 5 parts of thickener, 3 parts of hand wax powder, 3 parts of nano silicon dioxide dispersion, 1 part of water-based color essence, 1 part of wetting agent, 0.5 parts of defoamer, 1 part of dispersant and 20 parts of deionized water. The hand wax powder is polytetrafluoroethylene wax powder, the wetting agent is polyether silicone oil, the defoamer is polydimethylsiloxane, and the dispersant is polyacrylate ammonium salt dispersant.

[0058] The nano-matt paint for wooden floor is prepared by the following steps:

[0059] The matt resin obtained in Example 1 was stirred at a speed of 500 r / min, and a defoamer, a wetting agent, a dispersant and deionized water were added, and stirred at a speed of 900 r / min for 40 min. Then, hand wax powder, nano silicon dioxide dispersion and water-based color essence were added, and stirring was continued for 30 min. Finally, the thickener obtained in Example 4 was added, and stirring was continued for 15 min. The mixture was filtered to obtain a nano matt paint for wood floors.

[0060] Example 8

[0061] A nano matte paint for wood flooring includes the following raw materials by weight: 65 parts of matting resin, 6 parts of thickener, 4 parts of hand wax powder, 4 parts of nano silicon dioxide dispersion, 2 parts of water-based color essence, 1.5 parts of wetting agent, 0.7 parts of defoamer, 1.2 parts of dispersant and 25 parts of deionized water. The hand wax powder is polytetrafluoroethylene wax powder, the wetting agent is polyether silicone oil, the defoamer is polydimethylsiloxane, and the dispersant is polyacrylate ammonium salt dispersant.

[0062] The nano-matt paint for wooden floor is prepared by the following steps:

[0063] The matt resin obtained in Example 2 was stirred at a speed of 550 r / min, and a defoamer, a wetting agent, a dispersant and deionized water were added, and stirred at a speed of 950 r / min for 45 min. Then, hand wax powder, nano silicon dioxide dispersion and water-based color essence were added, and stirring was continued for 35 min. Finally, the thickener obtained in Example 5 was added, and stirring was continued for 25 min. The mixture was filtered to obtain a nano matt paint for wood floors.

[0064] Example 9

[0065] A nano matte paint for wood flooring includes the following raw materials by weight: 70 parts of matting resin, 7 parts of thickener, 5 parts of hand wax powder, 5 parts of nano silicon dioxide dispersion, 3 parts of water-based color essence, 2 parts of wetting agent, 1 part of defoamer, 1.5 parts of dispersant and 30 parts of deionized water. The hand wax powder is polytetrafluoroethylene wax powder, the wetting agent is polyether silicone oil, the defoamer is polydimethylsiloxane, and the dispersant is polyacrylate ammonium salt dispersant.

[0066] The nano-matt paint for wooden floor is prepared by the following steps:

[0067] The matt resin obtained in Example 3 was stirred at a speed of 600 r / min, and a defoamer, a wetting agent, a dispersant and deionized water were added, and stirred at a speed of 1000 r / min for 50 min. Then, hand wax powder, nano silicon dioxide dispersion and water-based color essence were added, and stirring was continued for 40 min. Finally, the thickener obtained in Example 6 was added, and stirring was continued for 30 min. The mixture was filtered to obtain a nano matt paint for wood floors.

[0068] Comparative Example 1

[0069] This comparative example is a commercially available nano-matt paint for wooden flooring.

[0070] Comparative Example 2

[0071] Compared with Example 9, the matting resin is replaced with ordinary water-based polyurethane and 4 parts of nano silicon dioxide are added as matting powder. The rest is exactly the same as Example 9 to prepare nano matt paint for wood flooring.

[0072] Comparative Example 3

[0073] Compared with Example 9, the intermediate a used in preparing the thickener is replaced with 11-bromo-undecanol, and the rest is exactly the same as Example 9 to prepare a nano-matt paint for wooden floors.

[0074] The effect of the nano-matt paint for wooden floor prepared by the present invention is further tested, and the test results are as follows.

[0075] In order to test the nano-matt paint for wood flooring prepared by the present invention, the performance was measured according to relevant standards, and the results are shown in Table 1.

[0076] Table 1:

[0077]

[0078] According to the data in Table 1, compared with Example 7, Example 8 and Example 9 and Comparative Example 1, it can be seen that compared with the commercially available nano matt paint for wood flooring, the nano matt paint for wood flooring prepared by the present invention has excellent toughness, adhesion, pencil hardness and water resistance; compared with the matt resin obtained by using the aqueous polyurethane introduced with epoxy resin modified terminal hydroxypropyl polydimethylsiloxane to participate in the copolymerization, the matt paint prepared by using only ordinary aqueous polyurethane and adding matting powder weakens the toughness, water resistance and adhesion of the matt paint; compared with the use of a thickener with a benzophenone structure, the use of a thickener without a benzophenone structure may cause the migration of the thickener, thereby reducing the toughness of the matt paint.

[0079] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A nano-matt paint for wooden floor, characterized by: The invention comprises the following raw materials in parts by weight: 60-70 parts of matting resin, 5-7 parts of thickener, 3-5 parts of hand wax powder, 3-5 parts of nano silicon dioxide dispersion, 1-3 parts of water-based color essence, 1-2 parts of wetting agent, 0.5-1 parts of defoaming agent, 1-1.5 parts of dispersant and 20-30 parts of deionized water; The matting resin used is prepared by the following steps: Step A1: Dry the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol at 100° C. in vacuum for 1 h and set aside for use. Add the terminal hydroxypropyl polydimethylsiloxane and polyethylene glycol to a flask equipped with a thermometer, a stirrer and a condenser, raise the temperature to 90° C., add toluene diisocyanate and dibutyltin disilicate under stirring, react at a constant temperature for 4 h, cool to 50° C., add 2,2-dihydroxymethylpropionic acid and tetrahydrofuran to the flask, raise the temperature to 70° C., react at a constant temperature for 2 h, and cool to room temperature to obtain intermediate 1; The amount ratio of terminal hydroxypropyl polydimethylsiloxane, polyethylene glycol, toluene diisocyanate, dibutyltin diisocyanate, 2,2-dihydroxymethylpropionic acid and tetrahydrofuran is 0.3 mol: 0.1 mol: 0.1-0.12 mol: 0.0015 mol: 0.002-0.003 mol: 250-300 mL; Step A2: under nitrogen protection, add bisphenol A epoxy resin E-12 to toluene, start stirring, slowly add intermediate 1 thereto, continue to react at 70-80° C. for 1-1.5 hours, wait until the system temperature drops to room temperature to obtain a reaction liquid, pour the reaction liquid into an emulsification barrel, add triethylamine and deionized water, and obtain intermediate 2 under high-speed stirring and shearing; The dosage ratio of bisphenol A epoxy resin E-12, toluene, intermediate 1, triethylamine and deionized water is: 0.1-0.13 g: 70 mL: 2-2.5 g: 0.08 g: 60 mL; Step A3: chitosan and diethylamine were added to the intermediate 2, and the mixture was stirred at 600 r / min and 60° C. for 5-6 h, and the temperature was lowered to 40° C., and pentaerythritol triacrylate was added, and the mixture was stirred for 3-4 h to obtain a matte resin; The usage ratio of intermediate 2, chitosan, diethylamine and pentaerythritol triacrylate is 2.6-3.0 g: 0.2-0.3 g: 0.5-0.6 g: 0.33-0.40 g; The thickener is prepared by the following steps: Step B1: Add 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF into a three-necked flask, stir and react at 80°C for 12h under nitrogen protection, extract with dichloromethane, dry and rotary evaporate to obtain intermediate a; The usage ratio of 2-hydroxy-4-n-octyloxybenzophenone, 11-bromo-undecanol, potassium carbonate and DMF is 0.15 mol: 0.18 mol: 0.30 mol: 50-60 mL; Step B2: Add polyethylene glycol and toluene to a flask, heat to 130°C under nitrogen protection, distill for 1.5-2h, cool to 60-70°C, add dibutyltin dilaurate and isophorone diisocyanate to the flask, stir and react at 80°C for 3.5-4h, then add intermediate a to the flask, stir and react at 85°C for 16h to obtain a mixed solution, cool the mixed solution to room temperature, recrystallize with ether, filter, add dichloromethane to the filter cake, and recrystallize with ether to obtain a thickener; The usage ratio of polyethylene glycol, toluene, dibutyltin dilaurate, isophorone diisocyanate and intermediate a is 0.25mmol:150mL:0.01g:2.5mmol:5mmol.

2. The nano-matt paint for wooden floor according to claim 1, characterized in that: The hand wax powder is polytetrafluoroethylene wax powder, the wetting agent is polyether silicone oil, the defoaming agent is polydimethylsiloxane, and the dispersant is polyacrylate ammonium salt dispersant.

3. The method for preparing a nano-matt paint for wooden floor according to claim 1, characterized in that: Made by the following steps: Stir the matt resin at a speed of 500-600r / min, add defoamer, wetting agent, dispersant and deionized water, stir at a speed of 900-1000r / min for 40-50min, then add hand wax powder, nano silica dispersion and water-based color essence, continue stirring for 30-40min, finally add thickener, continue stirring for 15-30min, filter, and you can get nano matt paint for wood floor.

Citation Information

Patent Citations

  • Modified water-based organic silicon polyurethane-polyacrylate nano hybrid waterborne coating free from VOC (volatile organic compound) chitosan and preparation method thereof

    CN103980791A

  • Photoreactive polyurethane associative thickener with benzophenone side group at tail end as well as preparation method and application thereof

    CN111944113A

  • Wear-resistant waterborne polyurethane matting coating material, preparation method and application thereof

    CN113105815A

  • Epoxy modified self-extinction waterborne polyurethane emulsion and preparation method thereof

    CN115058176A