A preparation method and application of supercapacitor electrode material
Two-dimensional porous nanomaterials were prepared by one-step hydrothermal method and magnetic stirring, combining polyvinylidene fluoride and acetylene black, and the complexity of electrode material preparation in the prior art was solved, and supercapacitor electrodes with high specific capacitance and capacitance retention were achieved Material.
Patent Information
- Application Number
- CN202410267510.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-08
AI Technical Summary
The preparation methods of existing supercapacitor electrode materials are complex, and multi-step synthesis methods may require templates and surfactants, which increase operational complexity and limited material application.
A one-step hydrothermal method is used to mix cobalt nitrate hexahydrate with urea, and two-dimensional porous nanomaterials are prepared by magnetic stirring and hydrothermal reaction, and then mixed with polyvinylidene fluoride and acetylene black, ground into an electrode slurry, coated on foam nickel On the other hand, high-specific capacitance electrode material was prepared by vacuum oven drying.
It realizes simple and easy preparation of two-dimensional porous nanomaterials, avoids the use of surfactants and templates, and the material has high specific capacitance and good capacitance retention, which is suitable for supercapacitors.
Smart Images

Figure CN117976429B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of supercapacitors, and in particular to a method for preparing a supercapacitor electrode material. Background Art
[0002] Supercapacitors are one of the most representative and widely used electrochemical energy storage devices. They have the characteristics of fast charging and discharging, long service life, and environmental friendliness. They have promoted the development of the new energy industry, especially in the field of electric vehicles. Due to the characteristics of cheap transition metal compounds and abundant content in the earth's crust, they have attracted public attention as electrode active materials. Different morphologies of electrode materials, such as nanoparticles, nanowires, nanospheres, microporous spheres, etc., have been widely reported. Different from the above morphological structures, two-dimensional nanostructures that can provide ion / electron transmission channels and stable structures have been prepared using different methods. However, most reports use multi-step synthesis methods to prepare nanosheet structure materials, which increases the complexity of the operation, or use a one-step method to prepare nanosheet structure materials with the help of templates or protective agents, which requires additional subsequent processing steps, limiting the application of the materials. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing an electrode material for a supercapacitor in view of the shortcomings of the prior art. The preparation method is simple, the preparation process is green and environmentally friendly, and the supercapacitor positive electrode material prepared by the method has a high specific capacitance.
[0004] In order to achieve the above object, the present invention adopts the following technical solution: a method for preparing a supercapacitor electrode material, comprising the following steps:
[0005] 1) gradually mixing cobalt nitrate hexahydrate and urea dispersion at a certain molar ratio, and mixing them by magnetic stirring to obtain a suspension;
[0006] 2) reacting the mixed system obtained in step 1) at room temperature for a period of time, and then adding ultrapure water to dilute it 10 times to obtain a dispersion;
[0007] 3) placing the dispersion obtained in step 2) in a high-temperature reactor with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0008] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water, and drying to obtain a light pink solid product;
[0009] 5) adding the light pink solid product obtained in step 4) to the mixture of polyvinylidene fluoride and acetylene black, grinding it evenly with a mortar, adding N-methylpyrrolidone dropwise and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor;
[0010] 6) uniformly coating the slurry obtained in step 5) on the cleaned nickel foam to obtain an electrode sheet;
[0011] 7) The electrode sheet prepared in step 6) was placed in a vacuum oven at 0.1 MPa, the temperature was set to 120° C., and dried for 12 h to obtain a working electrode.
[0012] Preferably, in step 1), the amount of cobalt nitrate hexahydrate is 0.035 mol, and the amount of cobalt nitrate hexahydrate to urea is 0.5:1 to 5:1, and the speed of magnetic stirring is 200-500 rpm / min.
[0013] Preferably, in step 1), the magnetic stirring treatment time is 1-30 hours.
[0014] Preferably, in step 2), the reaction is carried out at room temperature for 5-30 hours.
[0015] Preferably, in step 3), the volume ratio of ethanol to water is 1:1-6:1.
[0016] Preferably, in step 5), the mass ratio of light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, and the amount of N-methylpyrrolidone is 1-6 drops. The ultrasonic power is 100-150 W, the ultrasonic temperature is 16-28° C., and the ultrasonic time is 10-16 min.
[0017] Preferably, the nickel foam used in step 6) is first ultrasonically cleaned with dilute hydrochloric acid for 10 minutes, then cleaned with a mixture of ethanol and water in a volume ratio of 2:1 in an ultrasonic cleaner for 10 minutes, then cleaned with acetone for 10 minutes, and finally placed in an oven at 60° C. for drying for later use.
[0018] The invention also discloses the application of the supercapacitor electrode material. The specific capacitance of the material is 550-700 F / g.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] First, the method for preparing two-dimensional porous nanomaterials using a one-step hydrothermal method is simple, easy to operate, and has a large yield. Secondly, the two-dimensional porous nanomaterials prepared by this method do not require the use of any surfactants and templates, that is, no subsequent complex treatment methods are required. Finally, the two-dimensional porous nanomaterials prepared by this method have high specific capacitance when used as supercapacitor electrode materials (when the current density is 0.5A / g, the specific capacitance is 560F / g; when the current density increases to 10A / g, the capacitance retention rate can reach 79%). BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD pattern of prepared Co(OH)2 nanosheets.
[0022] Figure 2 SEM images of prepared Co(OH)2 nanosheets at different magnifications.
[0023] Figure 3 This is the cyclic voltammetry curve of the prepared Co(OH)2 nanosheets.
[0024] Figure 4 This is the constant current charge and discharge diagram for the preparation of Co(OH)2 nanosheets.
[0025] Figure 5 Impedance diagram of the prepared Co(OH)2 nanosheets. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0028] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0029] The present invention provides a method for preparing a supercapacitor electrode material. Cobalt nitrate hexahydrate is used as a metal salt, urea is used as a precipitant, and a one-step hydrothermal method without a template or surfactant is used to prepare a three-dimensional porous nanomaterial assembled from two-dimensional nanosheets. Then, the electrode material prepared above is loaded on nickel foam by a coating method to obtain a supercapacitor material with a higher specific capacitance-cobalt hydroxide nanomaterial.
[0030] Example 1
[0031] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0032] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.07 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 200 rpm / min, and the stirring time is 1 h;
[0033] 2) After the mixed system in step 1) reacts at room temperature for 5 hours, the suspension is diluted 10 times to obtain a dispersion;
[0034] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0035] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 1:1, and drying to obtain a light pink solid product;
[0036] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 1 drop of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0037] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0038] 7) Place the electrode sheet prepared in step 6) in a 0.1Mpa vacuum oven and set the temperature to 120
[0039] ℃, drying time is 12h, and the working electrode is obtained.
[0040] Example 2
[0041] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0042] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.0175 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 200 rpm / min, and the stirring time is 15 h;
[0043] 2) After the mixed system in step 1) reacts at room temperature for 5 hours, the suspension is diluted 10 times to obtain a dispersion;
[0044] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0045] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 3:1, and drying to obtain a light pink solid product;
[0046] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 3 drops of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0047] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0048] 7) The electrode sheet prepared in step 6) was placed in a vacuum oven at 0.1 MPa, the temperature was set to 120° C., and the drying time was 12 h to obtain a working electrode.
[0049] Example 3
[0050] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0051] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.0175 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 300 rpm / min, and the stirring time is 1 h;
[0052] 2) After the mixed system in step 1) reacts at room temperature for 15 hours, the suspension is diluted 10 times to obtain a dispersion;
[0053] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0054] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 3:1, and drying to obtain a light pink solid product;
[0055] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 3 drops of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0056] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0057] 7) The electrode sheet prepared in step 6) was placed in a vacuum oven at 0.1 MPa, the temperature was set to 120° C., and the drying time was 12 h to obtain a working electrode.
[0058] Example 4
[0059] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0060] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.012 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 300 rpm / min, and the stirring time is 1 h;
[0061] 2) After the mixed system in step 1) reacts at room temperature for 20 hours, the suspension is diluted 10 times to obtain a dispersion;
[0062] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0063] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 4:1, and drying to obtain a light pink solid product;
[0064] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 4 drops of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0065] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0066] 7) The electrode sheet prepared in step 6) was placed in a vacuum oven at 0.1 MPa, the temperature was set to 120° C., and the drying time was 12 h to obtain a working electrode.
[0067] Example 5
[0068] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0069] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.009 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 400 rpm / min, and the stirring time is 1 h;
[0070] 2) After the mixed system in step 1) reacts at room temperature for 25 hours, the suspension is diluted 10 times to obtain a dispersion;
[0071] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0072] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 3:1, and drying to obtain a light pink solid product;
[0073] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 5 drops of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0074] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0075] 7) The electrode sheet prepared in step 6) was placed in a vacuum oven at 0.1 MPa, the temperature was set to 120° C., and the drying time was 12 h to obtain a working electrode.
[0076] Example 6
[0077] A supercapacitor electrode material and a preparation method thereof, comprising the following steps:
[0078] 1) adding an aqueous solution of cobalt nitrate hexahydrate (0.035 mol, 30 mL) to an aqueous solution of urea (0.007 mol, 30 mL), and mixing the above solutions uniformly by magnetic stirring to obtain a mixed system, the magnetic stirring speed is 500 rpm / min, and the stirring time is 1 h;
[0079] 2) After the mixed system in step 1) reacts at room temperature for 30 hours, the suspension is diluted 10 times to obtain a dispersion;
[0080] 3) placing the dispersion obtained in step 2) in a high-temperature reaction kettle with a 50 mL inner container in an oven for hydrothermal reaction at a temperature of 180° C. for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product;
[0081] 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water in a volume ratio of 1:1, and drying to obtain a light pink solid product;
[0082] 5) adding the light pink solid product obtained in step 4) to a mixture of polyvinylidene fluoride and acetylene black, wherein the mass ratio of the light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, grinding it evenly with a mortar, adding 1 drop of N-methylpyrrolidone and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor.
[0083] 6) The electrode slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet.
[0084] 7) Place the electrode sheet prepared in step 6) in a 0.1Mpa vacuum oven and set the temperature to 120
[0085] ℃, drying time is 12h, and the working electrode is obtained.
[0086] Taking the material obtained in Example 6 as an experimental example, the present invention uses scanning electron microscopy (SEM) and X-ray diffraction (XRD) to characterize the supercapacitor electrode material as follows:
[0087] (1) Structural characterization
[0088] The structure of the three-dimensional porous material assembled from the prepared two-dimensional porous nanosheets was detected by D / max-γB type XRD. Figure 1 As shown. Figure 1It can be seen that the structure of the prepared nanomaterial is consistent with the standard card of Co(OH)2 nanomaterial, indicating that the supercapacitor electrode material was successfully prepared.
[0089] (2) Morphological characterization
[0090] The morphology of the prepared nanomaterials was characterized by S-4700 SEM. Figure 2 As shown in the figure, it can be seen that the morphology of the material is a three-dimensional porous structure assembled from two-dimensional nanosheets, and the thickness of the sheet is tens of nanometers.
[0091] (3) Cyclic voltammetry characterization
[0092] The performance of supercapacitors using the prepared materials as electrode materials was evaluated using cyclic voltammetry tests. Figure 3 As shown, it shows that the material is a capacitive hybrid material. In addition, at a larger scan rate, redox peaks still appear, indicating that the material is conducive to rapid reaction.
[0093] (4) Constant current charge and discharge test characterization
[0094] The performance of supercapacitors using the prepared materials as electrode materials was evaluated using constant current charge and discharge tests. Figure 4 As shown, the curves have similar charge and discharge platforms at all current densities, and the active material still has a high specific capacitance of 560 F / g at high current density.
[0095] (5) Impedance test
[0096] The ion transport and charge transfer impedance of the prepared active material were evaluated by electrochemical impedance spectroscopy, which showed that the material had low transport impedance and charge transfer impedance.
Claims
1. A method for preparing a supercapacitor electrode material, characterized in that: The following steps are involved: 1) gradually mixing cobalt nitrate hexahydrate and urea dispersion at a certain molar ratio, and mixing them by magnetic stirring to obtain a suspension; 2) reacting the mixed system obtained in step 1) at room temperature for a period of time, and then adding ultrapure water to dilute it 10 times to obtain a dispersion; 3) placing the dispersion obtained in step 2) in a high-temperature reactor with a 50 mL inner container and performing a hydrothermal reaction in an oven at a temperature of 180°C for 10 h. After the reaction is completed, washing and centrifugation are performed to obtain a pink flake product; 4) washing and separating the thin flake product after the reaction in step 3) with a mixture of ethanol and water, and drying to obtain a light pink solid product; 5) adding the light pink solid product obtained in step 4) to the mixture of polyvinylidene fluoride and acetylene black, grinding it evenly with a mortar, adding N-methylpyrrolidone dropwise and mixing it evenly under ultrasonic action to obtain an electrode slurry for a supercapacitor; 6) The slurry obtained in step 5) is evenly coated on the cleaned nickel foam to obtain an electrode sheet; 7) Place the electrode sheet prepared in step 6) in a vacuum oven at 0.1 Mpa, set the temperature to 120 °C, and dry for 12 hours to obtain a working electrode; In step 1), the amount of cobalt nitrate hexahydrate is 0.035 mol, and the amount of cobalt nitrate hexahydrate to urea is 0.5:1 to 5:1, and the speed of magnetic stirring is 200-500 rpm / min; In step 1), the magnetic stirring treatment time is 1-30 hours; In step 2), the reaction is carried out at room temperature for 5-30 hours; In step 4), the volume ratio of ethanol to water is 1:1-6:1; In step 5), the mass ratio of light pink solid product: polyvinylidene fluoride: acetylene black is 8:1:1, and the amount of N-methylpyrrolidone is 1-6 drops; the ultrasonic power is 100-150 W, the ultrasonic temperature is 16-28 °C, and the ultrasonic time is 10-16 min; The nickel foam used in step 6) is first ultrasonically cleaned with dilute hydrochloric acid for 10 min, then cleaned with a mixture of ethanol and water in a volume ratio of 2:1 in an ultrasonic cleaner for 10 min, then cleaned with acetone for 10 min, and finally placed in an oven at 60°C for drying for later use.
2. An electrode material, characterized in that: Prepared by the preparation method described in claim 1.
3. A use of the electrode material as claimed in claim 2, characterized in that: The specific capacitance of this electrode material is 550-700 F / g.