A low shrinkage acrylate vacuum impregnation agent for sealing reinforcement and preparation method thereof

By blending low viscosity acrylate monomers with secondary modified inorganic rigid particles in proton exchange membrane fuel cells, an impregnation reinforcement sealant with high filling rate was prepared, which solved the low filling rate and low filling rate in traditional methods. The problem of major pollution has achieved higher rigidity and sealing effect of graphite bipolar plates.

CN118006249BActive Publication Date: 2024-11-26NANJING AIBUNA SEALING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410408838.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-11-26
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

The reinforced sealant of traditional proton exchange membrane fuel cell graphite bipolar plates is contaminated due to limited filling rate, poor sealing effect and volatilization of organic solvents, resulting in low production efficiency and high pollution, making it difficult to meet the needs of high rigidity and airtightness.

Method used

Low-viscosity acrylate monomer is blended with secondary surface modified inorganic rigid particles, and an impregnation reinforcement sealant is prepared by high-speed centrifugal dispersion to avoid contamination of organic solvents and volume shrinkage, and improve filling rate and hardness.

Benefits of technology

It significantly improves the filling rate and sealing effect of graphite bipolar plates, reduces volume shrinkage before and after curing, enhances the rigidity and mechanical properties of the finished product, and solves the pollution and efficiency problems in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a low-shrinkage acrylate vacuum impregnating agent for sealing reinforcement and a preparation method thereof. The impregnating agent is obtained by uniformly mixing a monofunctional acrylate monomer, a difunctional acrylate monomer, a reactive emulsifier, secondary surface-modified inorganic rigid particles, an organic anti-shrinkage agent, an initiator and an inhibitor at room temperature. The impregnating agent has low viscosity and low toxicity. The gel time and the hardness of the glue stick after curing can meet the needs of industrial production. The impregnating agent has a volume shrinkage rate as low as 2-7%, and the hardness of the cured product is as high as 97 shoreA. The impregnating agent has the ability to efficiently block larger micropores, and has a high efficiency of blocking micropores at one time. The impregnating agent is an ideal impregnating agent for metal sealing reinforcement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a special impregnation reinforcing sealant which penetrates into the interior of a graphite bipolar plate of a proton exchange membrane fuel cell based on a pressure difference and generates a free radical polymerization reaction, wherein the sealant has the functions of plugging micropores of the graphite material, sealing the gas flow channel of the bipolar plate, and enhancing the mechanical strength of the graphite bipolar plate, in particular, the sealant is composed of a functional acrylate monomer and other additives. Background Art

[0002] The electrode plates commonly used in proton exchange membrane fuel cells are bipolar plates made of graphite materials through calendering, splitting and other steps, and gas flow channels are arranged on them. Because the graphite material itself is loose, there are a large number of micropores inside the finished product, which are prone to leakage when carrying gas circulation. Such micropores need to be filled and sealed to restore the air tightness of the electrode plate; at the same time, the graphite material is soft in texture, and the electrode plate is easy to deform and damage during installation, so a certain degree of reinforcement is needed to improve its hardness and rigidity.

[0003] Traditionally, porous and loose materials like graphite bipolar plates are processed by using sealing and reinforcing adhesives with organic solvents as carriers and unsaturated resins as effective components, such as phenolic resins, urea-formaldehyde resins, etc. The sealing and reinforcing adhesives are infiltrated into the micro-pores of the bipolar plates by impregnation, followed by desolventizing and curing. However, this type of unsaturated resin reinforcing adhesive has a considerable degree of volume shrinkage due to the need to remove the organic solvent as a carrier during the curing process, and has limited effect on filling and sealing micro-pores, requiring multiple impregnations to achieve the effect of sealing and reinforcement. The process of removing organic solvents during the production process can also cause volatile solvent pollution. The use of this type of unsaturated resin material to reinforce and seal graphite bipolar plates is highly polluting and inefficient, and this problem needs to be solved urgently. Summary of the invention

[0004] At present, the reinforcing sealant of graphite bipolar plates used in proton exchange membrane fuel cells often adopts unsaturated organic resin as the effective component and organic solvent as the carrier. In the production process, it has the disadvantages of limited filling rate, poor sealing effect, and pollution caused by volatilization of organic solvent.

[0005] The present invention provides an acrylate-based high-filling-rate impregnation reinforcing sealant for graphite bipolar plates of proton exchange membrane fuel cells, which has a low-viscosity acrylate monomer as a main component and inorganic rigid particles that have undergone secondary surface modification as an auxiliary filling component. Compared with traditional unsaturated polyester materials, it is an acrylate-based free radical reaction and bulk polymerization, and no organic solvent pollution is generated during the production process. At the same time, there is no mass loss during the polymerization and curing process, and the volume shrinkage is small. The method of secondary surface modification of inorganic rigid particles significantly improves the addition amount of inorganic rigid particles and the storage stability after addition; the method of blending with inorganic rigid particles, on the one hand, improves the hardness of the impregnation reinforcing sealant, thereby effectively improving the rigidity of the graphite bipolar plate after impregnation, and has a good reinforcement effect; on the other hand, it acts as a filler in the acrylate system, further reducing the shrinkage rate of the system before and after curing, improving the filling rate and sealing qualification rate of porous graphite materials, and improving the qualification rate in actual production.

[0006] The technical scheme of the present invention is divided into two stages: one is to perform secondary surface modification on inorganic rigid particles; the other is to use a high-speed centrifugal dispersion method to blend monofunctional acrylate, multifunctional acrylate, composite emulsifier, initiator, inhibitor and secondary modified inorganic rigid particles to prepare an impregnation reinforcement sealant for graphite bipolar plates of proton fuel cells.

[0007] Stage 1 is to modify the surface of inorganic rigid particles:

[0008] Step 1: treating the surface of the inorganic rigid particles with an interfacial compatibilizer / coupling agent, thereby obtaining inorganic rigid particles with treated surfaces and distributed with amino or acyl functional groups;

[0009] The inorganic rigid particles and the interfacial compatibilizer are mixed and stirred to form a mixture including the following components by weight:

[0010]

[0011] The specific steps for surface treatment of inorganic rigid particles are as follows:

[0012] The mixture is heated to 40-90° C. under sufficient stirring conditions, reacted for 60-360 minutes, filtered after cooling, and vacuum dried to obtain treated inorganic rigid particles.

[0013] The inorganic rigid particles refer to one or more of nano silicon dioxide, nano calcium carbonate, nano magnesium oxide and their commercial derivatives which have been surface treated with a coupling agent.

[0014] The interfacial compatibilizer refers to one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 2-aminoethyl 3-aminopropyltrimethoxysilane, and 2-aminoethyl 3-aminopropyltriethoxysilane.

[0015] Step 2: Use acid anhydride to treat the surface of inorganic rigid particles, and convert the amino or acyl groups distributed on the surface into carboxyl groups through grafting reaction, in preparation for secondary modification.

[0016] The modified inorganic rigid particles and the acid anhydride are mixed and stirred, and the specific composition is as follows:

[0017]

[0018] The specific steps for modifying the surface of inorganic rigid particles are as follows:

[0019] The mixture is heated to 40-90° C. under sufficient stirring conditions, reacted for 60-360 minutes, filtered after cooling, and vacuum dried to obtain inorganic rigid particles after carboxylation treatment.

[0020] The modified inorganic rigid particles refer to the inorganic rigid particles modified with an interfacial compatibilizer in step one.

[0021] The acid anhydride refers to one or more of phthalic anhydride, maleic anhydride and succinic anhydride.

[0022] Step three: Use a surfactant with a hydroxyl group at the polar end, blend it with the carboxyl-treated inorganic rigid particles, and undergo an esterification reaction with the carboxyl groups on the surface of the inorganic rigid particles through a grafting reaction, thereby grafting the surfactant molecules to the surface of the inorganic rigid particles to achieve the purpose of secondary modification.

[0023] The carboxylated inorganic rigid particles are dissolved and mixed with a surfactant, dispersed in a solvent with a relatively high boiling point (higher than water), mixed and stirred, and the specific composition is as follows:

[0024]

[0025] The specific steps for secondary modification of the surface of inorganic rigid particles are as follows:

[0026] Heat to 40-100°C under sufficient stirring, then evacuate the reaction container to a vacuum degree of 0.098-0.099MPa, remove the moisture generated in the reaction container by reduced pressure distillation, react for 60-420min, filter after cooling, and dry under reduced pressure in a vacuum box at a temperature of 40-60°C and a vacuum degree of 0.098-0.099MPa for 4-6h to obtain inorganic rigid particles that have undergone secondary modification.

[0027] The modified inorganic rigid particles refer to the inorganic rigid particles modified with anhydride in step 2.

[0028] The surfactant refers to a class of surfactants containing carboxyl or epoxy groups at the polar end, such as alkylphenol polyoxyethylene ether series (OP series), castor oil polyoxyethylene ether series (EL series), and polysorbate series (Tween series).

[0029] The solvent refers to one or more of toluene, xylene, pyridine, chlorobenzene, bromobenzene, 1,2-dibromoethane, aniline, dimethylformamide, dimethylacetamide, p-chlorotrifluorotoluene, and dimethyl sulfoxide.

[0030] Phase 2 is the preparation of impregnation reinforcement sealant for graphite bipolar plates of proton fuel cells. The technical solution is as follows:

[0031] The sealant is composed of monofunctional acrylate, multifunctional acrylate, composite emulsifier, secondary modified inorganic rigid particles, initiator, and inhibitor, and is mixed with the following components by mass:

[0032]

[0033] The raw materials are added into a stirring kettle according to a proportion, and mixed for 30-60 minutes to obtain an impregnation reinforcing sealant for graphite bipolar plates of proton exchange membrane fuel cells.

[0034] The monofunctional acrylate referred to is an alkyl ester of (meth)acrylic acid having 10 to 18 carbon atoms, such as one or more of lauryl acrylate, lauryl methacrylate, isodecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, tridecyl acrylate, and tridecyl methacrylate, or an alkyl ester of (meth)acrylic acid containing one or more hydroxyl functional groups, such as one or more of hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.

[0035] The multifunctional acrylate referred to is one or more of (meth) acrylate, 1,6-hexanediol diacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, 2-methyl-1,3-propanediol diacrylate, and 1,4-butanediol diacrylate.

[0036] The composite emulsifier referred to is one or more of polyoxyethylene sorbitan monooleate (TW-80), polyoxyethylene sorbitan monolaurate (TW-20), polyethylene glycol monooctylphenyl ether (OP-10), and castor oil polyoxyethylene ether (EL-40).

[0037] The secondarily modified inorganic rigid particles referred to are the secondarily modified inorganic rigid particles prepared in the first stage.

[0038] The initiator referred to is one of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, dibenzoyl peroxide, and cumene hydroperoxide.

[0039] The inhibitor referred to is one or more of hydroquinone, benzoquinone, naphthoquinone, anthraquinone, 2,6-dibutyl-p-cresol, picric acid, 4-methoxyphenol, naphthoquinone, phenothiazine, 2,6-di-tert-butylphenol, 2,5-di-tert-butylhydroquinone, 2,5-di-tert-butyl-1,4-benzoquinone, and 2,6-di-tert-butyl-4-ethylbenzoquinone.

[0040] The present invention adopts acrylate monomer and inorganic rigid particles that have been modified by secondary modification to prepare a high-efficiency impregnation reinforcement sealant for graphite bipolar plates of proton exchange membrane fuel cells. The acrylate monomer undergoes free radical reaction and bulk polymerization, and there is no solvent pollution and volume shrinkage problem of traditional unsaturated polyester reinforcement sealant. The use of inorganic rigid particles as fillers further reduces the volume shrinkage rate of the impregnation reinforcement sealant before and after curing, improves the filling rate of pores, and at the same time increases the hardness of the polymer after curing, thereby improving the rigidity of the finished graphite bipolar plate. The inorganic rigid particles are subjected to secondary modification, which increases the dispersibility and stability of the inorganic rigid particles in the acrylate system, and avoids the problems of agglomeration and sedimentation during storage caused by excessive addition. The principle of increasing the filling rate of inorganic rigid particles is that they replace part of the organic matter. Since this part of the inorganic rigid particles will not shrink, it is bound to be beneficial to the reduction of the volume shrinkage rate of the system; and since the compatibility of inorganic and organic matters is limited, an interface layer is formed at the interface between the inorganic rigid particles and the polymer after the polymer system is cured, which occupies a certain space, thereby being beneficial to the reduction of the volume shrinkage rate of the composite system. At the same time, the inorganic rigid particles will also form a sea-island structure in the molecular chain system after polymerization, which will have a steric effect, increase the rigidity of the molecular chain, and thus increase the hardness and rigidity of the finished graphite bipolar plate.

[0041] Traditional unsaturated polyester impregnation reinforcement sealant, due to its high viscosity, needs to be diluted with polar organic solvents during use to reduce its viscosity so as to facilitate its penetration into the porous graphite material; during the curing process, the solvent needs to be removed, resulting in a significant shrinkage of the sealant volume before and after curing, and a low filling rate for micro-pores, resulting in poor sealing effect and poor airtightness. At the same time, the graphite bipolar plates of proton exchange membrane fuel cells need to withstand a certain amount of pressure during installation, and there are certain requirements for the hardness of the finished product, but unsaturated polyester does not perform well in this regard.

[0042] The present invention uses an acrylate monomer and an inorganic rigid particle to mix to prepare an impregnation reinforcement sealant for a graphite bipolar plate of a proton exchange membrane fuel cell, thereby replacing the traditional unsaturated polyester sealant, solving the problems of gas pollution and volume shrinkage caused by the removal of organic solvents during the curing process of the traditional unsaturated polyester, and further improving the filling rate and reinforcement effect of the porous graphite material.

[0043] The impregnation reinforcement sealant is made of a pure acrylate base, with liquid acrylate as the main body. It does not need to use water or solvent to adjust the viscosity. Free radical polymerization occurs during the curing process, which belongs to bulk polymerization. There is no desolvation process, which reduces the volume shrinkage before and after curing. However, during the polymerization process, due to the characteristics of "slow initiation, fast growth, and fast termination" of the free radical reaction, the molecular weight will inevitably increase rapidly, forming regular long-chain polymers. Due to the natural trend of decreasing chemical potential in the system, they tend to be tightly and regularly arranged to form a tightly stacked structure, thereby significantly reducing the distance between molecules after polymerization. The macroscopic reaction is that the volume of the sealant still shrinks significantly after curing, so that its filling rate of fine pores still has certain defects. At the same time, the hardness of pure acrylate sealant after curing usually does not exceed 80 ShoreA, which cannot meet the reinforcement requirements of graphite bipolar plates. DETAILED DESCRIPTION

[0044] The specific implementation modes of the present invention are further explained in detail below through the description of embodiments, so as to help those skilled in the art to have a more complete, accurate and in-depth understanding of the inventive concept and technical solution of the present invention.

[0045] The present invention adds inorganic rigid particles to the selected acrylate monomers, which work together to reduce the volume shrinkage of the impregnation reinforcement sealant before and after curing, thereby increasing the filling rate of the pores. The test method for the volume shrinkage is tested by referring to the density method in GB / T 24148.9-2014.

[0046] Table 1 Comparison of volume shrinkage of typical sealant types

[0047]

[0048] Inorganic rigid particles do not react during the polymerization process and act as inert fillers. Their presence reduces shrinkage after polymerization. Because inorganic matter has limited compatibility in organic matter, inorganic rigid particles exist independently in the polymer after polymerization, with rigid particles as the core and chain polymers wrapped around the outside as the interface layer, forming a "sea-island" structure, which further destroys the tight stacking of the original regular long-chain polymers, reduces the distance between molecules, and macroscopically reduces the volume shrinkage before and after curing.

[0049] The main difficulty in adding inorganic rigid particles is that inorganic substances have limited compatibility in organic systems, and the viscosity of acrylate-based impregnation reinforcement sealants is low. After adding a large amount, it is easy to settle during storage, affecting the stability of the entire system. Some previous studies (Ling Xiao et al., China Adhesives 2012, 21 (1): 15-19) show that when the amount of inorganic rigid particles added exceeds 3%, sedimentation and turbidity are easy to occur in the sealant system. To solve this problem, three improvements are needed:

[0050] 1. After adding inorganic rigid particles, strengthen the stirring and dispersing process to disperse the inorganic rigid particles as evenly as possible to reduce the possibility of agglomeration and sedimentation;

[0051] 2. Surface modification of inorganic rigid particles or selection of commercial derivatives with appropriate surface modification;

[0052] 3. Appropriately increase the amount of emulsifier used and reuse multiple emulsifiers to ensure the dispersion stability of the system.

[0053] In terms of the process of strengthening stirring and dispersing, the traditional impregnation reinforcing sealant usually uses ordinary agitators and planetary agitators during the production process, which are very effective in dispersing low-viscosity liquids, but are not suitable for dispersing inorganic rigid particles. The solution is to use a high-speed centrifugal disperser, which has a centrifugal disk and is a multi-axis rotating centrifugal disperser. The agglomerated powder is evenly dispersed into the colloid by the stripping effect during the centrifugal rotation process. For example: the SH series of centrifugal nano-dispersers, the high-speed centrifuge disperses at a centrifugal speed of 1000-5000r / min. Take the addition of 10% mass fraction of nano-silicon dioxide to the surfactant-free acrylate monomer and leave it for 7 days to observe the effect as an example:

[0054]

[0055] It can be seen that after switching to high-speed centrifugal dispersion process, the uniform distribution and stability of inorganic rigid particles in the sealant have been greatly improved. Inorganic rigid particles with a mass fraction of 10% can also be evenly distributed in the acrylate monomer and remain stable for a period of time. Among them, the effect of increasing the centrifugal speed is more obvious, and extending the process time has a certain degree of improvement but cannot completely solve the sedimentation problem.

[0056] Due to the incompatibility between organic and inorganic substances, the higher the amount of inorganic rigid particles added, the higher the tendency of spontaneous agglomeration in the organic phase. Surface modification of inorganic rigid particles can graft / compound a layer of organic functional groups on their surface, increase their compatibility in the organic phase, and improve their distribution. Typically, silane coupling agent KH550 is added to nano-silica at a mass fraction of 3-5%, and dispersed and mixed with a solid mixer at 60°C for 2h. The treated nano-silica powder is added to the surfactant-free acrylate monomer at a mass fraction of 10%, and dispersed by high-speed centrifugation. The process of 2000r / min and 30min dispersion can achieve a no sedimentation effect within 7 days, and the dispersion stability is significantly improved. Some surface-modified rigid particles with better compatibility between the surface functional groups and the selected acrylate monomer, such as the gas-phase nano-silica HB-132 modified with hexamethyldioxysilazane, have equivalent or better effects.

[0057] Due to the incompatibility between organic and inorganic substances, the higher the amount of inorganic rigid particles added, the higher the tendency of spontaneous agglomeration in the organic phase. Surface modification of inorganic rigid particles can graft / compound a layer of organic functional groups on their surface to increase their compatibility in the organic phase and improve their distribution.

[0058] The common method in the prior art is: inorganic rigid particles are blended with coupling agents and interfacial compatibilizers having surface modification effects, and modified under heating and stirring conditions, so that a layer of organic matter with certain compatibility is attached to the surface of the inorganic rigid particles. This method can meet the requirements of increasing the compatibility of inorganic rigid particles to a certain extent, but the common interfacial compatibilizers such as KH550 used in the impregnation and reinforcement sealant for graphite bipolar plates for enhanced proton fuel cells have certain defects. The main reason is that the organic affinity end of common interfacial compatibilizers is usually an amino group or an acyl group, which has a strong polarity and is not compatible with the acrylate system. After adding a considerable amount of inorganic rigid particles to the system, agglomeration and sedimentation are prone to occur. The corresponding inorganic rigid particles are difficult to be tightly combined with acrylates, which has a certain adverse effect on the storage stability of the sealant and the anti-shrinkage effect of the sealant after curing.

[0059] The method for solving the above problem is to perform secondary modification on the inorganic rigid particles treated with an interfacial compatibilizer, firstly, an acid anhydride is used to undergo a grafting reaction with the organic end on the surface of the inorganic rigid particles, so that the organic end on the surface of the inorganic rigid particles is converted into a carboxyl group, and then a surfactant with a hydroxyl group or an epoxy group is reacted with the inorganic rigid particles with carboxyl groups on the surface to generate inorganic rigid particles with non-polar, oil-soluble surfactant branch ends on the outer surface. The inorganic rigid particles coated with the interfacial compatibilizer grafted with a surfactant having good oil solubility can be suspended in an acrylate system to form fine micelles, thereby obtaining good compatibility and dispersion effect in the acrylate system, and further increasing the amount of inorganic rigid particles added.

[0060] The reason why long-chain polymers are not commonly used in adhesives / sealants as an anti-shrinkage method is that long-chain polymers have good flexibility. When added to the acrylate system, they will reduce the hardness of the system after curing, weakening the sealing and reinforcement effects to a certain extent. At the same time, the long-chain polymer itself has a high viscosity. When added, it will increase the viscosity of the acrylate sealant system, which is not suitable for penetrating into the micro defects of the graphite bipolar plate during the subsequent sizing process.

[0061] Example 1

[0062] Stage 1: Preparation of secondary modified inorganic rigid particles

[0063] 1. Surface modification of inorganic rigid particles

[0064] 800 mesh nano-silica and interfacial compatibilizer 3-aminopropyltriethoxysilane (commercially available under the trade name KH-550) were mixed and stirred in water. The specific composition parts by mass are as follows:

[0065]

[0066] Heat to 50-53°C under sufficient stirring conditions, react for 120 minutes, filter after cooling, and vacuum dry. The reaction formula is as follows (not representing the actual volume ratio):

[0067]

[0068] Nano-silica particles 3-aminopropyltriethoxysilane

[0069]

[0070] Surface modified silica particles

[0071] 2. Surface carboxylation reaction

[0072] The surface-modified silica particles in the above step are mixed with succinic anhydride in water and stirred. The specific composition parts by mass are as follows:

[0073]

[0074] Heat to 68-73°C under sufficient stirring conditions, react for 120 minutes, filter after cooling, and vacuum dry. The reaction that occurs is the ring-opening grafting reaction of succinic anhydride and amine groups, and the reaction formula is as follows (does not represent the actual volume ratio):

[0075]

[0076] Surface modification of silica particles with succinic anhydride

[0077]

[0078] Surface carboxylated silica particles

[0079] 3. Secondary surface modification of inorganic rigid particles

[0080] The silicon dioxide particles with surface carboxylation in the above step are mixed with a surfactant, octanol polyoxyethylene (10) ether (trade name OP-10), in para-chlorotrifluorotoluene and stirred. The specific composition parts by mass are as follows:

[0081]

[0082] Heat to 80-83°C under sufficient stirring conditions, and continue to evacuate, keep the vacuum degree in the reactor at 0.098MPa-0.099MPa, react for 180 minutes, filter after cooling, and vacuum dry at 60°C. The reaction is an esterification reaction between the carboxyl group on the surface of the modified silica and the hydroxyl group at the polar end of OP-10. The reaction formula is as follows (does not represent the actual volume ratio):

[0083]

[0084] Surface carboxylated silica particle surfactant OP-10

[0085]

[0086] Secondary surface modified silica particles

[0087] Phase 2:

[0088] The following components are formulated into an impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells. The specific components are as follows by mass:

[0089]

[0090] After adding the components except the secondary surface-modified silica into the high-speed centrifugal disperser, start low-speed stirring and stir at 500r / min for 15 minutes to pre-mix the components. Then increase the speed to 5000r / min and add the modified silica into the centrifugal disperser twice. Maintain the current stirring speed for 10 minutes after each addition. Maintain the current stirring speed for another 10 minutes after all the materials are added.

[0091] For the graphite bipolar plate test piece, the main parameters are compared with the American counterparts Godfrey & Wing 95-1000A, the Japanese counterparts P-601E of Central Invention and the domestic product Nanjing Abner 8690 as follows.

[0092]

[0093] The test method for volume shrinkage is based on the density method in GB / T 24148.9-2014. The test method for hardness of cured products is based on the Shore durometer method specified in GB / T 2411. The test method for the first-time glue application pass rate is based on the standard test piece method specified in HG / T6100-2022. 50 typical graphite pressing test pieces are made for each group, and water tests are carried out under an air pressure of 0.33MPa. Leakage level ≤2 is considered qualified.

[0094] It can be seen that the finished product is significantly better than its peers in terms of volume shrinkage, and has a higher filling rate for the micropores of typical graphite specimens. This is reflected in the macroscopic view that the first-time sizing pass rate is significantly higher than that of peers. At the same time, its cured product has superior hardness, and its mechanical properties and aging resistance are not defective compared to peers. The finished product remains stable during the product's service life, without sedimentation or turbidity.

[0095] The above embodiments are only for illustrating the technical idea of ​​the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the present invention; any technology not involved in the present invention can be realized by existing technologies.

Claims

1. A method for preparing an impregnation reinforcing sealant for a proton fuel cell graphite bipolar plate, characterized in that: The sealant is composed of monofunctional acrylate, multifunctional acrylate, composite emulsifier, secondary modified inorganic rigid particles, initiator, and inhibitor, and is mixed by the following components in parts by mass: 50-85 parts of monofunctional acrylate, 20-55 parts of multifunctional acrylate, 5-20 parts of composite emulsifier, 5-20 parts of secondary modified inorganic rigid particles, 0.01-0.04 parts of initiator, 0.005-0.02 parts of inhibitor; The above components are added into a stirring kettle according to the proportions and mixed for 30-60 minutes to obtain an impregnation reinforcing sealant for graphite bipolar plates of proton exchange membrane fuel cells; The surface modification method of inorganic rigid particles comprises the following specific steps: Step 1: treating the surface of the inorganic rigid particles with an interfacial compatibilizer / coupling agent, thereby obtaining inorganic rigid particles with treated surfaces and distributed amino functional groups; The inorganic rigid particles and the interfacial compatibilizer are mixed and stirred to form a mixture of the following components by weight: 35-88 parts of inorganic rigid particles, 17-48 parts of interfacial compatibilizer, and 100-200 parts of water. The mixture is heated to 40-90° C. under sufficient stirring conditions, reacted for 60-360 minutes, filtered after cooling, and vacuum dried to obtain inorganic rigid particles with treated surfaces; The inorganic rigid particles refer to one or more of nano-silicon dioxide, nano-calcium carbonate, and nano-magnesium oxide; Step 2: Treat the surface of the inorganic rigid particles obtained in step 1 with anhydride, and convert the amino groups or acyl groups distributed on the surface into carboxyl groups through a grafting reaction, in preparation for secondary modification. The inorganic rigid particles obtained in step 1 are mixed with anhydride and stirred. The specific composition is as follows: 35-88 parts of inorganic rigid particles with treated surface, 4-17 parts of anhydride, and 100-200 parts of water. The specific steps for modifying the surface of inorganic rigid particles are as follows: The mixture is heated to 40-90° C. under sufficient stirring conditions, reacted for 60-360 minutes, filtered after cooling, and vacuum dried to obtain inorganic rigid particles that have been carboxylated; Step 3: using a surfactant with a hydroxyl group at the polar end, blending it with the inorganic rigid particles obtained in step 2, and undergoing an esterification reaction with the carboxyl groups on the surface of the inorganic rigid particles through a grafting reaction, thereby grafting the surfactant molecules onto the surface of the inorganic rigid particles to achieve the purpose of secondary modification; The inorganic rigid particles treated with carboxylation are dissolved and mixed with a surfactant, dispersed in a solvent having a boiling point higher than that of water, mixed and stirred, and the specific composition parts by mass are as follows: 35-88 parts of inorganic rigid particles treated with carboxylation, 2-25 parts of surfactant, and 100-200 parts of solvent. The specific steps for secondary modification of the surface of inorganic rigid particles are as follows: Heat to 40-100°C under sufficient stirring, then evacuate the reaction container to a vacuum degree of 0.098-0.099MPa, remove the moisture generated in the reaction container by reduced pressure distillation, react for 60-420min, filter after cooling, and dry under reduced pressure in a vacuum box at a temperature of 40-60°C and a vacuum degree of 0.098-0.099MPa for 4-6h to obtain inorganic rigid particles that have undergone secondary modification.

2. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The surfactant in step three is selected from one or more of alkylphenol polyoxyethylene ether series, castor oil polyoxyethylene ether series, and polysorbate series.

3. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The solvent in step three is selected from one or more of toluene, xylene, pyridine, chlorobenzene, bromobenzene, 1,2-dibromoethane, aniline, and dimethylformamide.

4. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The acid anhydride in step 2 is selected from one or more of phthalic anhydride, maleic anhydride and succinic anhydride.

5. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The interfacial compatibilizer in step 1 is selected from one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 2-aminoethyl 3-aminopropyltrimethoxysilane, and 2-aminoethyl 3-aminopropyltriethoxysilane.

6. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The monofunctional acrylate is an alkyl ester of (meth)acrylic acid having 10 to 18 carbon atoms, selected from one or more of lauryl acrylate, lauryl methacrylate, isodecyl methacrylate, octadecyl acrylate, octadecyl methacrylate, tridecyl acrylate, and tridecyl methacrylate, or an alkyl ester containing one or more hydroxyl functional groups in (meth)acrylic acid, selected from one or more of hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.

7. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The multifunctional acrylate is one or more selected from the group consisting of polyethylene glycol (meth)acrylate, 1,6-hexanediol diacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, 2-methyl-1,3-propanediol diacrylate, and 1,4-butanediol diacrylate.

8. The method for preparing the impregnation reinforcing sealant for graphite bipolar plates of proton fuel cells according to claim 1, characterized in that: The composite emulsifier is selected from one or more of polyoxyethylene sorbitan monooleate (TW-80), polyoxyethylene sorbitan monolaurate (TW-20), polyethylene glycol monooctylphenyl ether (OP-10), and castor oil polyoxyethylene ether (EL-40); the initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, dibenzoyl peroxide, and cumene hydroperoxide; the inhibitor is selected from one or more of hydroquinone, benzoquinone, naphthoquinone, anthraquinone, 2,6-dibutyl-p-cresol, picric acid, 4-methoxyphenol, naphthoquinone, phenothiazine, 2,6-di-tert-butylphenol, 2,5-di-tert-butylhydroquinone, 2,5-di-tert-butyl-1,4-benzoquinone, and 2,6-di-tert-butyl-4-ethylbenzoquinone.

9. The sealant prepared by the method for preparing the impregnation reinforcement sealant for graphite bipolar plates of proton fuel cells according to any one of claims 1 to 8.