Preparation method and application of a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst

By using magnetic biochar carriers to composite TiO2 and BiVO4 into photocatalysts, the problem of difficult separation and recovery of photocatalysts and poor resistance gene removal is achieved, achieving efficient photocatalytic performance and catalyst recovery, and significantly improving the efficiency of photocatalysts. Removal effect of resistance genes in aquaculture wastewater.

CN118022847BActive Publication Date: 2024-10-29BIOTECH CENT OF SHANDONG ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410299861.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-10-29
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

In practical applications, existing photocatalysts TiO2 and BiVO4 have problems such as low light utilization efficiency, easy electron-hole recombination, poor surface adsorption capacity, and difficulty in separation and recovery. Moreover, traditional sewage treatment technology has a negative impact on antibiotic resistance genes (ARGs). Removal effect is limited.

Method used

Magnetic biochar is prepared from agricultural and forestry solid waste as a carrier. The TiO2 and BiVO4 composite carrier is prepared into a quickly recyclable TiO2-MBC-BiVO4 composite photocatalyst through specific steps. The porous structure and conductivity of biochar are used to improve the photocatalytic performance. , and achieve effective separation and recovery of catalysts through the selection of magnetic biochar.

Benefits of technology

It improves the adsorption capacity of antagonistic genes, broadens the absorption spectrum range, increases light utilization, improves photocatalytic efficiency, and achieves effective separation and recovery of catalysts, significantly improving the removal effect of ARGs in aquaculture wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118022847B_ABST
    Figure CN118022847B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of photocatalysts, specifically a preparation method and application of a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered, comprising the following steps: preparing magnetic biochar; taking tetrabutyl titanate and putting it into anhydrous ethanol, stirring and mixing to obtain solution A; taking BiVO4 precursor and putting it into a mixed solvent, stirring and evenly obtaining solution B; dissolving a surfactant in anhydrous ethanol to obtain solution C; adding solution B and solution C to solution A at the same time under room temperature stirring, continuing to stir after the addition is completed, standing and aging to obtain a mixed solution; adding magnetic biochar to the mixed solution, stirring and dispersing evenly, aging to a gel state, drying to obtain a solid; pyrolyzing the solid, cooling to room temperature and then grinding and crushing to obtain a product. Composites of different materials are conducive to the rapid separation of electron-hole pairs, thereby improving the photocatalytic efficiency of the material. In addition, the photocatalytic material has magnetism, which is helpful for the effective separation and recovery of photocatalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalysts, and in particular to a preparation method and application of a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered. Background Art

[0002] my country is a major producer and user of antibiotics, with annual production accounting for about 60% of the world's total production and application accounting for about half of the world's total use. Among them, the use of antibiotics in livestock and poultry farming accounts for about 52% of the total use. However, the absorption and utilization rate of antibiotics in animals is low. About 70%-90% of antibiotics are discharged into the environment in the form of original drugs or metabolites with feces and urine, which puts great pressure on the environment. Antibiotics in the environment can induce microorganisms to produce antibiotic resistance genes (ARGs), making aquaculture wastewater a large repository of ARGs. ARGs can be transferred vertically between bacterial parent and offspring generations, or horizontally transferred within or between bacterial species through mobile genetic elements such as plasmids, integrons, and transposons, and have biological characteristics that can be replicated or spread. ARGs put pressure on microbial resistance, endanger human health, and are considered to be a new type of environmental pollutants.

[0003] Traditional sewage treatment technology can effectively reduce pathogenic microorganisms in water bodies, but the removal effect of ARGs is very limited. In recent years, advanced oxidation technology has achieved good results in ARGs wastewater treatment, especially photocatalytic technology has the advantages of simple equipment, easy operation, no secondary pollution, and wide application range, and is considered to be the most potential "green" water purification technology. Among them, the photocatalyst TiO2 is widely used due to its advantages such as low price and small side effects. However, its bandgap is about 3.2eV, and it only produces electron-hole pairs under the action of ultraviolet light, and the utilization rate of light is low. The bandgap of the photocatalyst BiVO4 is about 2.3-2.4eV, and it has absorption in both the ultraviolet and visible regions, but it has problems such as easy recombination of electrons and holes and poor surface adsorption capacity, resulting in its unsatisfactory photocatalytic performance. Moreover, as photocatalysts, TiO2 and BiVO4 have the problem of difficulty in separation and recovery in practical applications.

[0004] Existing technologies such as Chinese patent document CN 105944711 A (application number 201610283454.3) disclose a visible light responsive BiVO4 / TiO2 / graphene ternary composite photocatalyst and its preparation method, which combines BiVO4 and TiO2 for composite use, but it is mainly aimed at the treatment of organic dye pollutants. At the same time, this technology also does not solve the problem of catalyst separation and recovery during application. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a preparation method and application of a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered. In the preparation method, magnetic biochar prepared from agricultural and forestry solid waste is selected as a carrier, so that the prepared catalyst has good separation and recovery performance.

[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0007] A method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst comprises the following steps:

[0008] S1. The biomass material is washed, dried, and sieved to obtain biomass powder. The biomass powder is soaked in FeCl3 solution, filtered, dried, and pyrolyzed to obtain magnetic biochar (MBC);

[0009] S2. Tetrabutyl titanate was added to anhydrous ethanol and stirred to obtain solution A; Bi(NO3)3·5H2O and NH4VO3 in an equal molar ratio were added to a mixed solvent and stirred to obtain solution B; a surfactant was dissolved in anhydrous ethanol to obtain solution C;

[0010] S3. Solution B and solution C were simultaneously added dropwise to solution A under stirring at room temperature, and stirring was continued after the addition was completed, and the mixture was allowed to stand for aging to obtain a mixed solution;

[0011] S4. adding the magnetic biochar obtained in step S1 to the mixed solution obtained in step S3, stirring and dispersing the mixture evenly, aging the mixture into a gel state, and drying the gel in an oven to obtain a solid;

[0012] S5. The solid obtained in step S4 is pyrolyzed in an inert gas atmosphere, cooled to room temperature, and then ground and pulverized to obtain a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered.

[0013] Biochar (BC) is a carbon-rich material obtained by oxygen-limited pyrolysis of biomass materials such as agricultural and forestry waste and sludge. It has a special porous structure, high specific surface area and adsorption capacity, and can be used as a good catalyst carrier. By loading the photocatalyst on biochar by appropriate methods, the adsorption properties of biochar can be used to enhance the capture ability of pollutants. At the same time, the conductivity of carbon materials can also reduce the band gap energy of the photocatalyst, promote the rapid separation of photogenerated electron-hole pairs, and thus improve the photocatalytic performance of the composite material. In addition, the selection of magnetic biochar as a carrier will also help the effective separation and recovery of the photocatalyst.

[0014] Preferably, in step S1, the biomass material is crushed through a 100-mesh sieve to obtain biomass powder.

[0015] Preferably, in step S1, the concentration range of the FeCl3 solution is 0.5mol / L-2.0mol / L, and the soaking time is 1h-3h; further preferably, the concentration range of the FeCl3 solution is 1.0mol / L-1.5mol / L, and the soaking time is 2h-3h.

[0016] Preferably, in step S1, the ratio of biomass material to FeCl3 solution is 30g:(100-500)mL; further preferably, the ratio of biomass material to FeCl3 solution is 30g:(200-350)mL.

[0017] Preferably, in solution A of step S2, the volume ratio of tetrabutyl titanate to anhydrous ethanol is (2-3.5):5, and further preferably, the volume ratio of tetrabutyl titanate to anhydrous ethanol is 3:5.

[0018] Preferably, in solution B of step S2, the mixed solvent is formed by mixing mixed acid, deionized water and anhydrous ethanol in a volume ratio of 1: (1.3-1.9): 10, and the mixed acid is formed by mixing nitric acid and glacial acetic acid in a volume ratio of 1: (0.75-2); further preferably, the mixed solvent is formed by mixing mixed acid, deionized water and anhydrous ethanol in a volume ratio of 1: 1.5: 10, and the mixed acid is formed by mixing nitric acid and glacial acetic acid in a volume ratio of 1: 1.5.

[0019] Preferably, in solution B of step S2, the addition ratio of Bi(NO3)3·5H2O to the mixed acid is (0.008-0.012) mol:1 mL; further preferably, the addition ratio of Bi(NO3)3·5H2O to the mixed acid is 0.01 mol:1 mL.

[0020] Preferably, in solution C of step S2, the surfactant is selected from one or more of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, Tween, etc., the dosage of the surfactant is 1-5% of the mass of tetrabutyl titanate converted to the Ti element, and the ratio of the surfactant to anhydrous ethanol is (0.01-0.05) g:5 mL; further preferably, the surfactant is hexadecyltrimethylammonium bromide, the dosage of the surfactant is 3% of the mass of tetrabutyl titanate converted to the Ti element, and the ratio of the surfactant to anhydrous ethanol is 0.03 g:5 mL.

[0021] Preferably, in step S3, the ratio of the molar amount of Bi element in solution B to the molar amount of Ti element in solution A is in the range of (0.55-1.12):1, the volume ratio of solution B to solution A is (0.9-1.5):1, and the dropping speed of solution B and solution C is 1 drop / s; further preferably, the ratio of the molar amount of Bi element in solution B to the molar amount of Ti element in solution A is in the range of (0.65-1):1, and the volume ratio of solution B to solution A is (1-1.2):1.

[0022] Preferably, in step S3, the stirring time is 1.5-3h, the static aging temperature is 25-30°C, and the static aging time is 6-12h; further preferably, the stirring time is 2h, the static aging temperature is 25°C, and the static aging time is 8h.

[0023] Preferably, in step S4, the ratio of the added mass of magnetic biochar to the mass of Ti element in the mixed solution obtained in step S3 is (1-5):1; further preferably, the ratio of the added mass of magnetic biochar to the mass of Ti element in the mixed solution obtained in step S3 is (2.5-4):1.

[0024] Preferably, in step S4, the aging temperature is 25-30°C, and the aging time is 24-60h; further preferably, the static aging temperature is 25°C, and the static aging time is 48h.

[0025] Preferably, in step S5, the inert gas is selected from one of nitrogen, helium or argon, and the pyrolysis is specifically carried out by heating the temperature to 300-700°C at a rate of 2-10°C / min and maintaining the temperature for 0.5-4h; further preferably, the pyrolysis is specifically carried out by heating the temperature to 500°C at a rate of 5°C / min and maintaining the temperature for 1h.

[0026] Preferably, in step S5, the solid is ground in a mortar and pulverized through a 100-200 mesh sieve; more preferably, the solid is ground through a 200 mesh sieve.

[0027] The present invention also provides the use of the rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared by the above preparation method in removing resistance genes in aquaculture wastewater.

[0028] Preferably, in the application, the rapidly recoverable TiO2-MBC-BiVO4 composite photocatalyst is added into the wastewater containing the resistance gene in the range of 0.05-0.15 g / L, and the resistance gene is removed under visible light conditions.

[0029] The beneficial effects of the present invention are:

[0030] (1) The agricultural and forestry solid waste used in the present invention is widely available, cheap and easy to obtain, and can be used on a large scale to achieve resource utilization and achieve the purpose of "using waste to treat pollution".

[0031] (2) The photocatalytic material prepared by the present invention has simple process and operation, does not require special equipment, and is easy to realize industrial production.

[0032] (3) The composite photocatalytic material prepared by the present invention improves the adsorption capacity of ARGs, broadens the absorption spectrum range, and increases the light utilization rate. At the same time, the composite of different materials is also conducive to the rapid separation of electron-hole pairs, thereby improving the photocatalytic efficiency of the material. In addition, the magnetic properties of the photocatalytic material are conducive to the effective separation and recovery of the photocatalyst.

[0033] (4) The composite photocatalytic material prepared by the present invention is green, non-toxic and environmentally friendly.

[0034] (5) The composite photocatalytic material prepared by the present invention has a good removal effect on ARGs in aquaculture wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The X-ray diffraction pattern of the rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared in Example 1;

[0036] Figure 2 This is a SEM image of the rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared in Example 1;

[0037] Figure 3 This is the hysteresis loop of the rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared in Example 1. DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with embodiments and drawings.

[0039] The present invention provides a method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst, comprising the following steps:

[0040] S1. The biomass material is washed, dried and sieved to obtain biomass powder, and the biomass powder is soaked in FeCl3 solution, filtered, dried and pyrolyzed to obtain magnetic biochar (MBC);

[0041] S2. Tetrabutyl titanate was added to anhydrous ethanol and stirred to obtain solution A; Bi(NO3)3·5H2O and NH4VO3 in an equal molar ratio were added to a mixed solvent and stirred to obtain solution B; a surfactant was dissolved in anhydrous ethanol to obtain solution C;

[0042] S3. Solution B and solution C were simultaneously added dropwise to solution A under stirring at room temperature, and stirring was continued after the addition was completed, and the mixture was allowed to stand for aging to obtain a mixed solution;

[0043] S4. adding the magnetic biochar obtained in step S1 to the mixed solution obtained in step S3, stirring and dispersing the mixture evenly, aging the mixture into a gel state, and drying the gel in an oven to obtain a solid;

[0044] S5. The solid obtained in step S4 is pyrolyzed in an inert gas atmosphere, cooled to room temperature, and then ground and pulverized to obtain a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered.

[0045] The present invention also provides the use of the rapidly recoverable TiO2-MBC-BiVO4 composite photocatalyst prepared by the above preparation method in removing ARGs from aquaculture wastewater. The rapidly recoverable TiO2-MBC-BiVO4 composite photocatalyst is added into the wastewater containing resistance genes in the range of 0.05-0.15 g / L, and the ARGs are treated under visible light conditions.

[0046] In the prior art, many preparation processes for preparing magnetic biochar have been disclosed, such as patent CN117205907A (application number 202311179254.X), which also uses biomass as raw material and uses co-precipitation method to prepare magnetic biochar-titanium dioxide composite materials. However, the magnetic biochar prepared by co-precipitation method has magnetic particles precipitated on the surface of biochar, which is not firmly bonded and easily falls off. The preparation method provided in this application can generate magnetic particles in situ on the surface and pores of biochar, which is more firmly bonded and not easy to fall off during application and recycling, and can maintain good and stable magnetism.

[0047] Example 1

[0048] A method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst comprises the following steps:

[0049] S1. The peanut shells were cleaned with deionized water, dried at 75 ° C for 24 h, crushed and passed through a 100-mesh sieve to obtain peanut shell powder, and then 30 g of peanut shell powder was soaked in 350 mL of 1 mol / L FeCl3 solution for 3 h, filtered, naturally dried, and pyrolyzed to obtain MBC;

[0050] S2. Slowly add 6 ml of tetrabutyl titanate to 10 ml of anhydrous ethanol, stir magnetically to mix well, and obtain solution A; mix 0.4 ml of nitric acid, 0.6 ml of glacial acetic acid, 1.5 ml of deionized water and 10 ml of anhydrous ethanol, then add 5.8 g of Bi(NO3)3·5H2O and 1.4 g of NH4VO3, stir magnetically until mixed well, and obtain solution B. Dissolve 0.03 g of hexadecyltrimethylammonium bromide in 5 ml of anhydrous ethanol to obtain solution C;

[0051] S3. At room temperature, equal volumes of solution B and solution C were slowly added dropwise to solution A under continuous magnetic stirring at a rate of about 1 drop / second. After the addition was complete, stirring was continued for 2 hours, and then the mixture was allowed to stand at room temperature for 8 hours to obtain a mixed solution.

[0052] S4. 2.5 g of magnetic biochar was added to the mixed solution and uniformly dispersed in the mixed solution, and aged at 25° C. for 48 h to form a gel solid;

[0053] S5. Pyrolyze the gel solid in a nitrogen atmosphere furnace, raise the temperature to 500°C at a rate of 5°C / min, maintain it for 1 hour, and then cool it to room temperature. Grind the obtained solid and pass it through a 200-mesh sieve to obtain a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered.

[0054] The rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared above was tested by X-ray diffraction, and the results were as follows Figure 1 As shown in the figure, we can see the characteristic diffraction peaks of TiO2, BiVO4, Fe3O4, and the characteristic peaks of amorphous carbon, which shows that the composite material contains all of the above substances. Figure 2 As shown in the figure, the results show that TiO2 and BiVO4 are successfully loaded on the surface and voids of biochar. Figure 3 As shown, this indicates that the composite material has certain magnetic properties and can be quickly recovered under the action of an external magnetic field.

[0055] Example 2

[0056] A method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst comprises the following steps:

[0057] S1. The corn stalks were cleaned with deionized water, dried at 75°C for 24 h, crushed and passed through a 100-mesh sieve to obtain corn stalk powder, and then 30 g of corn stalk powder was soaked in 200 mL of 1.5 mol / L FeCl3 solution for 1 h, filtered, naturally dried, and pyrolyzed to obtain MBC;

[0058] S2. 7 ml of tetrabutyl titanate was slowly added to 10 ml of anhydrous ethanol, and the mixture was uniformly mixed under magnetic stirring to obtain solution A; 0.4 ml of nitric acid, 0.4 ml of glacial acetic acid, 1.2 ml of deionized water and 8 ml of anhydrous ethanol were uniformly mixed, and then 4.64 g of Bi(NO3)3·5H2O and 1.12 g of NH4VO3 were added, and the mixture was uniformly mixed under magnetic stirring to obtain solution B; 0.049 g of hexadecyltrimethylammonium bromide was dissolved in 5 ml of anhydrous ethanol to obtain solution C;

[0059] S3. Solution B and solution C were slowly added dropwise to solution A under continuous magnetic stirring at a volume ratio of 1.2:1 at room temperature, and the drop rate was controlled at about 1 drop / second. After the addition was completed, stirring was continued for 2 hours, and then the mixture was allowed to stand at room temperature for 12 hours to obtain a mixed solution;

[0060] S4. 4.93 g of magnetic biochar was added to the mixed solution and uniformly dispersed in the mixed solution, and aged at 30° C. for 60 h to form a gel solid;

[0061] S5. The gel solid was pyrolyzed in an argon atmosphere furnace, heated to 700°C at a rate of 10°C / min, maintained for 4 hours and then cooled to room temperature. The obtained solid was ground and sieved through a 200-mesh sieve to obtain a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered.

[0062] Example 3

[0063] A method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst comprises the following steps:

[0064] S1. The pig manure was dried at 75°C for 24 hours, crushed and passed through a 100-mesh sieve to obtain pig manure powder, and then 30 g of the pig manure powder was soaked in 100 mL of 1.25 mol / L FeCl3 solution for 3 hours, filtered, naturally dried, and pyrolyzed to obtain MBC;

[0065] S2. Slowly add 4 ml of tetrabutyl titanate to 10 ml of anhydrous ethanol, stir magnetically to mix well, and obtain solution A; mix 0.4 ml of nitric acid, 0.3 ml of glacial acetic acid, 0.91 ml of deionized water and 7 ml of anhydrous ethanol, then add 4.06 g of Bi(NO3)3·5H2O and 0.98 g of NH4VO3, stir magnetically until mixed well, and obtain solution B; dissolve 0.006 g of hexadecyltrimethylammonium bromide in 5 ml of anhydrous ethanol to obtain solution C;

[0066] S3. Solution B and solution C were slowly added dropwise to solution A under continuous magnetic stirring at a volume ratio of 1.1:1 at room temperature, and the drop rate was controlled at about 1 drop / second. After the addition was completed, stirring was continued for 1.5 hours, and then the mixture was allowed to stand at room temperature for 6 hours to obtain a mixed solution;

[0067] S4. 0.56 g of magnetic pig manure biochar was added to the mixed solution and uniformly dispersed in the mixed solution, and aged at 30° C. for 24 h to form a gel solid;

[0068] S5. Pyrolyze the gel solid in an argon atmosphere furnace, raise the temperature to 300°C at a rate of 2°C / min, maintain it for 4 hours, and then cool it to room temperature. Grind the obtained solid and pass it through a 200-mesh sieve to obtain a TiO2-MBC-BiVO4 composite photocatalyst that can be quickly recovered.

[0069] Comparative Example 1

[0070] A method for preparing a TiO2-MBC-BiVO4 composite photocatalyst is provided according to the method provided in Example 1 in Chinese patent document CN 105944711A, except that an equal amount of magnetic biochar prepared in step S1 of Example 1 is used instead of graphene oxide to prepare the TiO2-MBC-BiVO4 visible light catalytic composite material.

[0071] Comparative Example 2

[0072] A method for preparing a TiO2-MBC-BiVO4 composite photocatalyst. The difference between this comparative example and Example 1 is that in step S2, an equal amount of nitric acid is used instead of a mixed acid of nitric acid and glacial acetic acid to prepare the TiO2-MBC-BiVO4 composite photocatalyst.

[0073] Comparative Example 3

[0074] A method for preparing a TiO2-MBC-BiVO4 composite photocatalyst. The difference between this comparative example and Example 1 is that in step S2, the amount of deionized water added is 2.5 ml, and the amount of other substances added remains unchanged.

[0075] Comparative Example 4

[0076] A method for preparing a TiO2-MBC-BiVO4 composite photocatalyst. The difference between this comparative example and Example 1 is that in step S3, the ratio of the molar amount of the Bi element in solution B to the molar amount of the Ti element in solution A is 2.2:1, and the dosages of Bi(NO3)3·5H2O and NH4VO3 are adjusted accordingly to prepare the TiO2-MBC-BiVO4 composite photocatalyst.

[0077] Comparative Example 5

[0078] A method for preparing a TiO2-MBC-BiVO4 composite photocatalyst. The difference between this comparative example and Example 1 is that in step S4, the dosage of magnetic biochar is 0.3g, and the dosage of other substances remains unchanged to prepare the TiO2-MBC-BiVO4 composite photocatalyst.

[0079] Experimental example

[0080] The rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared in each embodiment and the TiO2-MBC-BiVO4 composite photocatalyst prepared in each comparative example were used to carry out an experiment to remove resistance genes in aquaculture wastewater, and the steps are as follows:

[0081] Take 30 ml of each solution containing different concentrations of tetracycline resistance gene (tetA) and ampicillin resistance gene (Amp), set up two parallel groups, add 30 mg of the photocatalytic material prepared in Example 1 and Comparative Example 1 respectively, and carry out photocatalytic reaction for 2 hours. The catalytic reaction device is equipped with a xenon lamp with a power of 0-500 W and an ultraviolet filter to ensure that the visible light source radiates to each reaction container. After the reaction is completed, the two composite photocatalytic materials are quickly separated from the solution by an external magnetic field, and the concentrations of tetracycline resistance gene (tetA) and ampicillin resistance gene (Amp) in the solution are measured again, and the removal rate of the two resistance genes and the recovery rate of the composite photocatalytic material are calculated. The results are shown in Table 1.

[0082] Table 1 The removal effect of each prepared composite photocatalytic material on resistance genes and its corresponding recovery rate

[0083]

[0084] As can be seen from the above table, the photocatalyst prepared in Example 1 has a high removal rate of 99.3% and 99.5% for tetracycline resistance gene (tetA) and ampicillin resistance gene (Amp) in aquaculture wastewater, respectively. The removal rates of the photocatalysts prepared in Examples 2 and 3 for the two resistance genes are slightly reduced but still higher than 95%; while the photocatalyst prepared in Comparative Example 1 has a removal rate of 68.5% and 69.8% for the two resistance genes, respectively. Although the removal rates of the photocatalysts prepared in Comparative Examples 2-5 for the two resistance genes are significantly lower than those prepared in Example 1, the removal rates are higher than those prepared in Comparative Example 1. This is because BiVO4 and TiO2 in the present invention are both generated in situ on the surface of magnetic biochar during the reaction process, and the combination of the three is more closely distributed and more uniform, which is conducive to the electron transport in the photocatalytic process and the inhibition of the recombination of electron-hole pairs, thereby improving the photocatalytic effect. However, in Comparative Example 1, the preparation of BiVO4 alone and then physical mixing with TiO2 and magnetic biochar is not conducive to improving the photocatalytic effect.

[0085] After the photocatalytic reaction is completed, the photocatalyst is quickly separated, collected and dried, and the recovery rate is calculated. The results show that in the experiment of treating two resistance genes, the recovery rates of the photocatalyst prepared in Example 1 are 96.8% and 95.5%, respectively, and the recovery rates of the photocatalysts prepared in Example 2 and Example 3 are also higher than 95%, while the recovery rate of the photocatalyst prepared in Comparative Example 1 is only 71.7% and 72%. The recovery rates of the photocatalysts prepared in Comparative Examples 2-5 are not less than 85%, which is higher than that of Comparative Example 1. This is because BiVO4 and TiO2 in the present invention are both generated in situ on the surface of the magnetic biochar during the reaction process, and the three are combined into a whole and are not easy to fall off. In Comparative Example 1, BiVO4 is first prepared separately and then physically mixed with TiO2 and magnetic biochar. The three are not tightly combined and are easy to fall off during recovery, resulting in a low recovery rate.

Claims

1. A method for preparing a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst, characterized in that: The steps include: S1. The biomass material is washed, dried, and sieved to obtain biomass powder, and the biomass powder is soaked in FeCl3 solution, filtered, dried, and pyrolyzed to obtain magnetic biochar MBC; S2. Tetrabutyl titanate was added to anhydrous ethanol and stirred to obtain solution A; Bi(NO3)3·5H2O and NH4VO3 in an equal molar ratio were added to a mixed solvent and stirred to obtain solution B; a surfactant was dissolved in anhydrous ethanol to obtain solution C; S3. Solution B and solution C were simultaneously added dropwise to solution A under stirring at room temperature, and stirring was continued after the addition was completed, and the mixture was allowed to stand for aging to obtain a mixed solution; S4. Add the magnetic biochar MBC obtained in step S1 to the mixed solution obtained in step S3, stir and disperse evenly, and then age it into a gel state, and dry the gel in an oven to obtain a solid; S5. The solid obtained in step S4 is pyrolyzed under an inert gas atmosphere, cooled to room temperature, and then ground and crushed to obtain a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst; BiVO4 and TiO2 are both generated in situ on the surface of magnetic biochar MBC, and TiO2 and BiVO4 are loaded onto the surface and voids of magnetic biochar MBC.

2. The preparation method according to claim 1, characterized in that In step S1, the concentration range of the FeCl3 solution is 0.5 mol / L-2.0 mol / L, and the soaking time is 1 h-3 h.

3. The preparation method according to claim 2, characterized in that: In step S1, the concentration range of the FeCl3 solution is 1.0 mol / L-1.5 mol / L, and the soaking time is 2h-3h.

4. The preparation method according to claim 1, characterized in that: In step S1, the ratio of biomass material to FeCl3 solution is 30g:(100-500)mL.

5. The preparation method according to claim 4, characterized in that: In step S1, the ratio of biomass material to FeCl3 solution is 30g:(200-350)mL.

6. The preparation method according to claim 1, characterized in that: In the solution A of step S2, the volume ratio of tetrabutyl titanate to anhydrous ethanol is (2-3.5):5; In the solution B of step S2, the mixed solvent is prepared by mixing mixed acid, deionized water and anhydrous ethanol in a volume ratio of 1:(1.3-1.9):10, the mixed acid is prepared by mixing nitric acid and glacial acetic acid in a volume ratio of 1:(0.75-2), and the addition ratio of Bi(NO3)3·5H2O to the mixed acid is (0.008-0.012) mol:1 mL; In the solution C of step S2, the surfactant is selected from one or more of sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium bromide or Tween, the dosage of the surfactant is 1-5% of the mass of tetrabutyl titanate converted to Ti element, and the ratio of the surfactant to anhydrous ethanol is (0.01-0.05) g:5 mL.

7. The preparation method according to claim 6, characterized in that: In the solution A of step S2, the volume ratio of tetrabutyl titanate to anhydrous ethanol is 3:5; In the solution B of step S2, the mixed solvent is prepared by mixing mixed acid, deionized water and anhydrous ethanol in a volume ratio of 1:1.5:10, and the mixed acid is prepared by mixing nitric acid and glacial acetic acid in a volume ratio of 1:1.5; the addition ratio of Bi(NO3)3·5H2O to the mixed acid is 0.01 mol:1 mL; In the solution C of step S2, the surfactant is hexadecyltrimethylammonium bromide, the dosage of the surfactant is 3% of the mass of tetrabutyl titanate converted to Ti element, and the ratio of the surfactant to anhydrous ethanol is 0.03 g:5 mL.

8. The preparation method according to claim 1, characterized in that: In step S3, the ratio of the molar amount of Bi element in solution B to the molar amount of Ti element in solution A is in the range of (0.55-1.12):1, the volume ratio of solution B to solution A is (0.9-1.5):1, and the dropping speed of solution B and solution C is 1 drop / s.

9. The preparation method according to claim 8, characterized in that: In step S3, the ratio of the molar amount of Bi element in solution B to the molar amount of Ti element in solution A is in the range of (0.65-1):1, and the volume ratio of solution B to solution A is (1-1.2):

1.

10. The preparation method according to claim 1, characterized in that: In step S3, the stirring time is 1.5-3 hours, the temperature for static aging is 25-30° C., and the static aging time is 6-12 hours.

11. The preparation method according to claim 10, characterized in that: In step S3, the stirring time is 2 hours, the temperature for static aging is 25° C., and the static aging time is 8 hours.

12. The preparation method according to claim 1, characterized in that: In step S4, the ratio of the added mass of magnetic biochar MBC to the mass of Ti element in the mixed solution obtained in step S3 is (1-5):1; in step S4, the aging temperature is 25-30°C, and the aging time is 24-60h.

13. The preparation method according to claim 12, characterized in that: In step S4, the ratio of the added mass of magnetic biochar MBC to the mass of Ti element in the mixed solution obtained in step S3 is (2.5-4):1; the aging temperature is 25° C., and the aging time is 48 h.

14. The preparation method according to claim 1, characterized in that: In step S5, the inert gas is selected from one of nitrogen, helium or argon, and the pyrolysis is specifically carried out by heating to 300-700°C at a rate of 2-10°C / min and then maintaining for 0.5-4h; in step S5, the solid is ground in a mortar and crushed through a 100-200 mesh sieve.

15. The preparation method according to claim 14, characterized in that: In step S5, the pyrolysis is specifically carried out by heating the mixture to 500°C at a rate of 5°C / min and then maintaining the temperature for 1 hour; and grinding the mixture to pass through a 200-mesh sieve.

16. Use of a rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst prepared by the preparation method according to any one of claims 1 to 15 in removing resistance genes from aquaculture wastewater.

17. The use according to claim 16, characterized in that The rapidly recyclable TiO2-MBC-BiVO4 composite photocatalyst was added into the wastewater containing the resistance gene in the range of 0.05-0.15 g / L, and the resistance gene was removed under visible light conditions.

Citation Information

Patent Citations

  • Visible-light-responsive BiVO4 / TiO2 / graphene tri-material composite light catalyst and preparation method thereof

    CN105944711A

  • Magnetic charcoal-titanium dioxide composite material as well as preparation method and application thereof