A modified anti-cutting coating glove with both good hand feel and wear resistance and preparation method thereof

By using bio-based surfactant modified aramid pulp and nitrile latex to prepare impregnated latex and adding silk peptide powder, the problem of rough surface and insufficient wear resistance of nitrile glossy gloves is solved, and the resistance of gloves is improved Wear and feel improve the wearable experience.

CN118027754BActive Publication Date: 2024-11-22JIANGSU HANVO SAFETY PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410029055.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-09
Publication Date
2024-11-22
Estimated Expiration
2044-01-09

AI Technical Summary

Technical Problem

The surface of nitrile glossy anti-cut gloves is rough and not smooth due to the presence of aramid pulp, resulting in poor wear experience and insufficient wear resistance.

Method used

Immersed latex are prepared by bio-based surfactant-modified aramid pulp and nitrile latex. Gloves are prepared by impregnation and vulcanization treatment, and silk peptide powder is added to enhance the wear resistance and feel of the coating.

Benefits of technology

It significantly improves the wear resistance and feel of the gloves, making the surface delicate and smooth, improving the wear experience, and improving the wear resistance of the gloves.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a modified anti-cutting coated glove with both hand feeling and wear resistance and a preparation method, comprising a glove core and an impregnated latex coated on the outer layer of the glove core, wherein the impregnated latex comprises the following raw materials in parts by weight: 90-120 parts of nitrile latex, 0.6-1.1 parts of KOH, 1-3 parts of surfactant, 1-2 parts of sulfur, 2-5 parts of zinc oxide, 1-7 parts of silk peptide powder, 2-6 parts of kaolin, 4-7 parts of modified aramid pulp, and 1-2 parts of black pigment. The present invention has the advantages that the surface of the prepared gloves is delicate and smooth, the hand feeling of the gloves is comprehensively improved, and the wear resistance of the coating is also improved to a certain extent, thereby improving the wearing experience of the user.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glove preparation, and in particular to a modified anti-cutting coated glove having both good hand feel and wear resistance and a preparation method thereof. Background Art

[0002] Nitrile smooth cut-resistant gloves are highly favored in the labor protection gloves market due to their excellent functions such as chemical resistance, oil resistance, and cut resistance. Cut-resistant nitrile smooth gloves have a wide range of applications due to their durable coating surface and certain cut-resistant functions; however, after the nitrile smooth coating has certain cut-resistant properties, due to the presence of aramid pulp, its surface is not smooth and the back cover is hard, making the wearing experience very poor.

[0003] Aramid pulp modified with bio-based surfactants is added to latex and processed through dipping and other processes to produce finished gloves, which comprehensively improves the anti-cutting performance and wear resistance; modified aramid pulp, as a rubber reinforcing agent, can greatly improve the strength, hardness and wear resistance of rubber products, and can also improve the ductility and elasticity of rubber products. However, the surface coating of gloves made of this modified aramid pulp has a certain roughness, and the user experience is lacking. Summary of the invention

[0004] The purpose of the present invention is to provide a modified anti-cutting coated glove with both good hand feel and wear resistance and a preparation method thereof. The surface of the prepared glove is delicate and smooth, the hand feel of the glove is comprehensively improved, and the wear resistance of the coating is also improved to a certain extent, thereby improving the wearing experience of the user.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions:

[0006] A modified anti-cut coated glove with both hand feel and wear resistance, characterized in that it comprises a glove core and an impregnated latex coated on the outer layer of the glove core, wherein the impregnated latex comprises the following raw materials in parts by weight: 90 to 120 parts of nitrile latex, 0.6 to 1.1 parts of KOH, 1 to 3 parts of a surfactant, 1 to 2 parts of sulfur, 2 to 5 parts of zinc oxide, 1 to 7 parts of silk peptide powder, 2 to 6 parts of kaolin, 4 to 7 parts of modified aramid pulp, and 1 to 2 parts of black pigment.

[0007] Preferably, the surfactant is sodium tripolyphosphate.

[0008] A method for preparing a modified cut-resistant coated glove having both good hand feel and wear resistance, characterized in that it comprises the following steps:

[0009] S1, taking aramid fibers, pre-cleaning them, drying and sealing them, and obtaining aramid pulp;

[0010] S2, preparing a bio-based surfactant, adding aramid pulp thereto and mixing evenly to obtain an aramid dispersion, then adding an anti-settling agent to the aramid dispersion, and standing at room temperature for 8 hours to obtain a modified aramid pulp;

[0011] S3, adding all the raw materials by weight and mixing them to prepare the impregnated latex;

[0012] S4, taking the glove core and putting it on the hand mold for preheating;

[0013] S5, taking the preheated glove core and dipping it into the coagulant;

[0014] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0015] S7. After the rubber surface of the glove core is formed, pre-vulcanization and high-temperature vulcanization treatment are performed for 1 hour each;

[0016] S8, demoulding, obtaining gloves.

[0017] Preferably, the aramid fiber pre-cleaning in S1 is specifically soaking in an acetone solution for 2 hours to remove surface impurities, washing with deionized water, and drying in a 45° C. oven for 4 hours.

[0018] Preferably, the aramid fiber in S1 is aramid 1414 fiber.

[0019] Preferably, the bio-based surfactant in S2 is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, and the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g.

[0020] Preferably, the preheating temperature in S4 is 60°C.

[0021] Preferably, the coagulant in S5 is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3% to 10%.

[0022] Preferably, the pre-vulcanization temperature in S7 is 90°C and the high-temperature vulcanization temperature is 110°C.

[0023] In summary, the beneficial effects of the present invention are:

[0024] 1. The carbonyl compound in silk peptide powder reacts with the carbonylamine compound in the amino compound to make the macromolecular polymerization denser, thereby improving the wear resistance of the coating. The silk protein in silk peptide powder has excellent compatibility. During the coating treatment process, it is tightly combined with the coating material through intermolecular forces, which greatly improves the wear resistance of the coating and makes the coating surface more delicate and smooth.

[0025] 2. After silk peptide powder is added to the coating formula, the finished gloves are made through processes such as dipping. The surface of the gloves is delicate and smooth, the feel of the gloves is comprehensively improved, and the wear resistance of the coating is also improved to a certain extent, which improves the previous poor feel of the gloves and enhances the wearing experience of the users. DETAILED DESCRIPTION

[0026] The specific implementation modes of the present invention are further described below, and these embodiments do not constitute a limitation of the present invention.

[0027] Example 1

[0028] S1. Soak aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, seal and set aside after drying to obtain aramid pulp.

[0029] S2. Prepare a bio-based surfactant sodium tripolyphosphate, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0030] S3, prepare dipping latex; by weight, including the following raw materials: 90 parts of nitrile latex, 0.6 parts of KOH, 2 parts of surfactant sodium tripolyphosphate, 1 part of sulfur, 3 parts of zinc oxide, 1 part of silk peptide powder, 3 parts of kaolin, 5 parts of modified aramid pulp, and 1 part of black pigment;

[0031] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0032] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%;

[0033] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0034] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0035] S8, demoulding, obtaining gloves.

[0036] Example 2

[0037] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0038] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0039] S3, prepare dipping latex; by weight, including the following raw materials: 90 parts of nitrile latex, 0.6 parts of KOH, 1 part of surfactant sodium tripolyphosphate, 1 part of sulfur, 2 parts of zinc oxide, 2 parts of silk peptide powder, 3 parts of kaolin, 5 parts of modified aramid pulp, and 1 part of black pigment;

[0040] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0041] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%;

[0042] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0043] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0044] S8, demoulding, obtaining gloves.

[0045] Example 3

[0046] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0047] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0048] S3, prepare dipping latex; by weight, including the following raw materials: 100 parts of nitrile latex, 1.0 parts of KOH, 3 parts of surfactant sodium tripolyphosphate, 2 parts of sulfur, 4 parts of zinc oxide, 3 parts of silk peptide powder, 6 parts of kaolin, 5 parts of modified aramid pulp, and 1 part of black pigment;

[0049] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0050] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 3%;

[0051] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0052] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0053] S8, demoulding, obtaining gloves.

[0054] Example 4

[0055] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0056] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0057] S3, prepare dipping latex; by weight, including the following raw materials: 120 parts of nitrile latex, 1.1 parts of KOH, 3 parts of surfactant sodium tripolyphosphate, 2 parts of sulfur, 5 parts of zinc oxide, 4 parts of silk peptide powder, 3 parts of kaolin, 7 parts of modified aramid pulp, and 2 parts of black pigment;

[0058] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0059] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 5%;

[0060] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0061] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0062] S8, demoulding, obtaining gloves.

[0063] Example 5

[0064] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0065] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0066] S3, prepare dipping latex; by weight, including the following raw materials: 90 parts of nitrile latex, 0.6 parts of KOH, 1 part of surfactant sodium tripolyphosphate, 2 parts of sulfur, 2 parts of zinc oxide, 5 parts of silk peptide powder, 5 parts of kaolin, 4 parts of modified aramid pulp, and 1 part of black pigment;

[0067] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0068] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 5%;

[0069] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0070] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0071] S8, demoulding, obtaining gloves.

[0072] Example 6

[0073] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0074] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0075] S3, prepare dipping latex; by weight, including the following raw materials: 100 parts of nitrile latex, 0.8 parts of KOH, 2 parts of surfactant sodium tripolyphosphate, 1 part of sulfur, 3 parts of zinc oxide, 6 parts of silk peptide powder, 3 parts of kaolin, 5 parts of modified aramid pulp, and 1 part of black pigment;

[0076] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0077] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 7%;

[0078] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0079] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0080] S8, demoulding, obtaining gloves.

[0081] Example 7

[0082] S1. Soak the aramid 1414 fiber in acetone solution for 2 hours to remove surface impurities, wash with deionized water, dry in a 45°C oven for 4 hours, and seal for later use after drying;

[0083] S2. Prepare a bio-based surfactant, add aramid pulp into it and mix evenly to obtain an aramid dispersion, then take an anti-settling agent and add it to the aramid dispersion, the bio-based surfactant is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g, let it stand at room temperature for 8h, and obtain modified aramid pulp;

[0084] S3, prepare dipping latex; by weight, including the following raw materials: 100 parts of nitrile latex, 0.8 parts of KOH, 2 parts of surfactant sodium tripolyphosphate, 1 part of sulfur, 3 parts of zinc oxide, 7 parts of silk peptide powder, 3 parts of kaolin, 5 parts of modified aramid pulp, and 1 part of black pigment;

[0085] S4, take the glove core and put it on the hand mold, and preheat it at a temperature of 60°C;

[0086] S5, taking the glove core of step S2 and dipping it into a coagulant, wherein the coagulant is a mixture of acetic acid and methanol, and the volume fraction of acetic acid in the mixture is 10%;

[0087] S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature;

[0088] S7, perform pre-vulcanization at 90°C and high-temperature vulcanization at 110°C for 1 hour each;

[0089] S8, demoulding, obtaining gloves.

[0090] Comparative Example 1

[0091] The difference from Example 1 is that no silk peptide powder is added.

[0092] The mechanical properties of gloves are tested using the European standard EN-388 test method.

[0093] Glove finger slip is measured by dry slip method, the weight is 1.5kg, and the standard unit of finger slip is (kgf).

[0094] The above-mentioned Examples 1-7 and Comparative Example 1 were subjected to mechanical test analysis, and the specific test results are shown in Table 1 below:

[0095] Table 1 Mechanical test results of various embodiments and comparative examples

[0096] Cut Resistant Wear-resistant Finger Slide Tear puncture Example 1 Level 1 (8500r) Level 4 (2.9)LL Level 3 Level 1 Example 2 Level 1 (8700r) Level 4 (2.8)LL Level 3 Level 1 Example 3 Level 1 (9000r) Level 4 (2.7)LL Level 3 Level 1 Example 4 Level 1 (9500r) Level 4 (2.6)LL Level 3 Level 1 Example 5 Level 1 (12000r) Level 4 (2.5)LL Level 3 Level 1 Example 6 Level 1 (13500r) Level 4 (2.4)LL Level 3 Level 1 Example 7 Level 1 (14000r) Level 4 (2.2)LL Level 3 Level 1 Comparative Example 1 Level 1 (8300r) Level 4 (3.0)LL Level 3 Level 1

[0097] It can be seen from the above experimental data that the treatment method provided by the present invention can effectively improve the wear resistance of gloves. Silk peptide powder is mainly composed of silk protein and sericin, wherein silk protein is connected by an H chain with a molecular weight of about 350,000 and an L chain with a molecular weight of about 27,000. The H chain is formed by a crystalline region formed by repeating the amino acid arrangement sequence of Gly-Ala-Gly-Ala-Gly-Ser / Tyr, and a non-crystalline region formed by disordered arrangement of amino acids. These four amino acids account for more than 90% of the amino acid species of silk protein. The crystalline region adopts a β-sheet structure, forming a strong interchain interaction to form a fiber, and sericin plays a role in covering the silk protein. The carbonyl compound in the silk peptide powder reacts with the amino compound to make the macromolecular polymerization more dense, thereby improving the wear resistance of the coating; the silk protein in the silk peptide powder has excellent compatibility, and in the coating treatment process, it is closely combined with the coating material through intermolecular forces, which greatly improves the wear resistance of the coating, and makes the coating surface more delicate and smooth. After silk peptide powder is added to the coating formula, the finished gloves are made through processes such as dipping. The surface of the gloves is delicate and smooth, the feel of the gloves is comprehensively improved, and the wear resistance of the coating is also improved to a certain extent, which improves the previous poor feel of the gloves and enhances the wearing experience of the users.

[0098] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions should also be deemed to fall within the protection scope of the technical solution of the present invention.

Claims

1. A modified cut-resistant coated glove having both good hand feel and wear resistance, characterized in that: It comprises a glove core and an impregnated latex coated on the outer layer of the glove core, wherein the impregnated latex comprises the following raw materials in parts by weight: 90-120 parts of nitrile latex, 0.6-1.1 parts of KOH, 1-3 parts of a surfactant, 1-2 parts of sulfur, 2-5 parts of zinc oxide, 1-7 parts of silk peptide powder, 2-6 parts of kaolin, 4-7 parts of modified aramid pulp, and 1-2 parts of black pigment; The preparation method comprises the following steps: S1, taking aramid fibers, pre-cleaning them, drying and sealing them, and obtaining aramid pulp; S2, preparing a bio-based surfactant, adding aramid pulp thereto and mixing evenly to obtain an aramid dispersion, then adding an anti-settling agent to the aramid dispersion, and standing at room temperature for 8 hours to obtain a modified aramid pulp; S3, adding all the raw materials by weight and mixing them to prepare the impregnated latex; S4, taking the glove core and putting it on the hand mold for preheating; S5, taking the preheated glove core and dipping it into the coagulant; S6, take the glove core and immerse it in the dipping latex, and spread the latex at room temperature; S7. After the rubber surface of the glove core is formed, pre-vulcanization and high-temperature vulcanization are performed for 1 hour each, the pre-vulcanization temperature is 90°C, and the high-temperature vulcanization temperature is 110°C; S8, demoulding, obtaining gloves.

2. The modified cut-resistant coated glove having both good hand feel and good wear resistance according to claim 1, characterized in that: The surfactant is sodium tripolyphosphate.

3. The modified cut-resistant coated glove having both good hand feel and good wear resistance according to claim 1, characterized in that: The aramid fiber pre-cleaning in S1 is specifically to immerse it in an acetone solution for 2 hours to remove surface impurities, wash it with deionized water, and then dry it in a 45° C. oven for 4 hours.

4. The modified cut-resistant coated glove having both good hand feel and good wear resistance according to claim 1, characterized in that: The aramid fiber in S1 is aramid 1414 fiber.

5. The modified cut-resistant coated glove having both good hand feel and good wear resistance according to claim 1, characterized in that: The bio-based surfactant in S2 is a rhamnolipid solution with a mass fraction of 5%, the anti-settling agent is a sodium carboxymethyl cellulose aqueous solution with a mass fraction of 2%, and the volume mass ratio of the bio-based surfactant, aramid pulp and anti-settling agent is 1L:100g:20g.

6. The modified cut-resistant coated glove having both good hand feel and good wear resistance according to claim 1, characterized in that: The preheating temperature in S4 is 60°C.