A wear-resistant and heat-insulating card protection film and preparation process

By introducing sodium sulfonate and silicone groups into the protective film for copolyesterization, the modified polyethylene terephthalate base layer is formed, which solves the thermal insulation, wear resistance and anti-static of the protective film. The problem of insufficient performance achieves better heat insulation, wear resistance and anti-static effects, and extends service life.

CN118027833BActive Publication Date: 2024-11-08HUIZHOU YIDU STATIONERY SUPPLIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410151533.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-11-08
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

The existing card protection film has shortcomings in thermal insulation, wear resistance and antistatic properties, which leads to deformation, bending and contamination in high-temperature environments, which affects service life.

Method used

Sodium sulfonate group and silicone group are used to prepare sodium sulfonate silicone monomer through chemical reaction, and copolyesterized with polyethylene terephthalate to form modified polyterephthalate. The ethylene glycol formate base layer is coated with polyethylene and ethylene-vinyl acetate copolymer layers on the base layer in turn, and a wear-resistant and heat-insulating guard film is prepared by corona treatment and extrusion process.

Benefits of technology

It significantly improves the thermal insulation, wear resistance and antistatic properties of the card protection film, extends the service life and broadens its application areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118027833B_ABST
    Figure CN118027833B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of card protection films, and discloses a wear-resistant and heat-insulating card protection film and a preparation process thereof. The synthesized sodium dicarboxylate sulfonate organic silicon monomer is similar to the molecular structure of polyethylene terephthalate, and is easy to combine with each other, thereby improving the interface compatibility. The modified polyethylene terephthalate base layer has a Si-O-Si structure, and forms a highly cross-linked interpenetrating network structure similar to silicon dioxide during melt solidification, and has good wear resistance. At the same time, the silicon-oxygen bonds in its molecular chain have high thermal stability, so that the gas molecules in the base layer cannot convect, and a continuous insulation layer is formed, thereby having a good heat insulation effect. In addition, the antistatic sodium sulfonate group has hygroscopicity and ion conductivity, so that its molecular chain can penetrate the base layer of the card protection film to form a conductive channel, and is not easy to migrate to the polymer surface, thereby making the antistatic performance of the card protection film lasting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of card protection films, in particular to a wear-resistant and heat-insulating card protection film and a preparation process thereof. Background Art

[0002] Card protection film is a protective film that is applied as a base film to the outer surface of a card to isolate and protect the card and make it easier to pack the card. It is also called plastic sealing film or laminating film. It is generally a sheet packaging material with a polyester film as the base layer, an adhesive coated on the base layer, and special processing. It is widely used for the sealing and protection of various sheet materials such as identity cards, historical materials, photos and pictures. It has the functions of waterproofing, anti-tampering, moisture-proofing and anti-mildew. However, the existing card protection film has certain shortcomings in terms of heat insulation. Excessively high temperature or long-term high temperature environment will cause the card protection film itself to deform, and the existing card protection film is very easy to bend during use, which brings certain damage to the sheet material that needs to be protected by its plastic sealing. Therefore, the development of a multifunctional card protection film has become a hot topic of current research.

[0003] The existing card protection film structure is usually composed of a polyethylene terephthalate (PET) film layer, a polyethylene film layer and an ethylene-vinyl acetate copolymer film layer. Polyethylene terephthalate has good film transparency and high transparency, which makes it easy for people to identify patterns or texts on the card. However, due to the insulating properties of PET itself, static charges are easily generated and accumulated during contact and friction, making the surface of the PET card protection film easy to absorb dust during storage and use, affecting the appearance effect; at the same time, since the card protection film is touched and used for a long time, these documents and cards are very easy to be contaminated and damaged, which indirectly affects the service life of the card protection film; however, the card protection film prepared by the prior art has poor thermal insulation performance, and its antistatic and wear resistance are also poor, which limits the further use of the card protection film.

[0004] The present invention adopts a method for modifying the PET film base layer of the card protection film, prepares a sodium dicarboxylic acid sulfonate organosilicon monomer through a chemical reaction of a functional sodium sulfonate group and a siloxane group, and then polycondenses the monomer with ethylene glycol to obtain a sodium sulfonate organosilicon copolyester with a structure similar to that of the PET film base layer, thereby improving the thermal insulation performance of the card protection film while increasing its wear resistance and antistatic properties, further broadening the application field of the card protection film. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, provide a wear-resistant and heat-insulating card protection film and a preparation process, and solve the problems of poor heat insulation performance and poor wear resistance of the existing card protection film.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A preparation process of a wear-resistant and heat-insulating card protection film, wherein the structure of the card protection film is, from the inner layer to the outer layer, an ethylene-vinyl acetate copolymer adhesive layer, a polyethylene layer and a modified polyethylene terephthalate base layer, and the preparation process comprises the following steps:

[0008] (1) After drying polyethylene terephthalate and sodium sulfonate silicone copolyester in a vacuum drying oven at a temperature of 110-130° C. for 12-24 hours, adding the mixture into a high-speed mixer, then adding an antioxidant, stirring the mixture evenly, and then melt-extruded the mixture on a twin-screw extruder, water-cooled and pelletized to obtain modified polyethylene terephthalate.

[0009] (2) After the modified polyethylene terephthalate is melted, it is biaxially stretched to obtain a polyester film layer, and then corona treatment is performed by a corona machine. Then, the polyethylene is melted, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller to obtain a wear-resistant and heat-insulating card protection film.

[0010] Preferably, in step (1), the ratio of polyethylene terephthalate, sodium sulfonate organosilicon copolyester and antioxidant is 100g:8-25g:0.1-0.5g.

[0011] Preferably, in step (1), the temperatures of the barrel sections of the twin-screw extruder are 280-300°C, 305-320°C, 310-325°C, and 290-310°C, respectively, and the screw speed is 60-100 r / min.

[0012] Preferably, the preparation process of sodium sulfonate organosilicon copolyester comprises the following steps:

[0013] S1. Add N,N-dimethylformamide and p-aminobenzoic acid into a reaction flask, stir evenly, then add sodium 3-chloro-2-hydroxypropane sulfonate and cesium carbonate, stir for reaction, and after the reaction is completed, concentrate under reduced pressure, recrystallize in ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate.

[0014] S2. Add dimethyldichlorosilane and toluene to the reaction flask, stir evenly, add 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate sodium and triethylamine, stir to react, and after the reaction is completed, concentrate under reduced pressure, recrystallize in ethanol aqueous solution, and dry to obtain a molecule with the structural formula: Sodium dicarboxylate sulfonate silicone monomer.

[0015] S3. Add terephthalic acid, sodium dicarboxylate sulfonate organosilicon monomer, ethylene glycol and tetrabutyl titanate into a reaction flask, stir evenly at 220-250° C. under a nitrogen atmosphere, heat to 255-270° C. for polycondensation reaction, the reaction time is 2-7 hours, cool and discharge to obtain sodium sulfonate organosilicon copolyester.

[0016] Preferably, in step S1, the ratio of p-aminobenzoic acid, N,N-dimethylformamide, sodium 3-chloro-2-hydroxypropane sulfonate, and cesium carbonate is 1 mol: 2000-2500 mL: 0.85-1.0 mol: 1.5-2.5 mol.

[0017] Preferably, in step S1, the reaction temperature is 130-150° C., and the reaction time is 5-10 h.

[0018] Preferably, in step S2, the ratio of dimethyldichlorosilane, toluene, sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate, and triethylamine is 1 mol: 1500-2000 mL: 2.05-2.3 mol: 2.2-3.5 mol.

[0019] Preferably, in step S2, the reaction temperature is 55-70° C. and the reaction time is 2-6 h.

[0020] Preferably, in step S3, the ratio of terephthalic acid, sodium dicarboxylic acid sulfonate organosilicon monomer, ethylene glycol, and tetrabutyl titanate is 0.7-0.92 mol: 0.08-0.30 mol: 1.6-2.0 mol: 0.0015-0.003 mol.

[0021] By adopting the above technical solution, the beneficial effects of the present invention are:

[0022] The invention synthesizes functional dicarboxylic acid monomers. Firstly, p-aminobenzoic acid, sodium 3-chloro-2-hydroxypropane sulfonate and cesium carbonate are reacted to obtain sodium 3-((4-carboxylphenyl)amino)-2-hydroxypropane-1-sulfonate. Then, a substitution reaction is carried out with dimethyldichlorosilane to obtain sodium dicarboxylic acid sulfonate organic silicon monomer. Then, an esterification polycondensation reaction is carried out with ethylene glycol to obtain modified polyethylene terephthalate. Then, the polyethylene terephthalate and the sodium sulfonate organic silicon copolyester are blended and extruded to obtain a modified polyethylene terephthalate base layer. The base layer is subjected to surface corona treatment. A polyethylene layer and an ethylene-vinyl acetate copolymer adhesive layer are sequentially coated on the base layer to obtain a wear-resistant and heat-insulating card protection film.

[0023] Since the molecular structure of sodium dicarboxylic acid sulfonate silicone monomer is basically the same as that of polyethylene terephthalate, they are easy to combine with each other, which improves the interface compatibility. The modified polyethylene terephthalate base layer has a Si-O-Si structure, and a highly cross-linked interpenetrating network structure similar to silicon dioxide is formed during melt solidification, which has good wear resistance and is beneficial to improving the adhesion between the surface layers of the card protection film, thereby obtaining a base material with excellent wear resistance. At the same time, the silicon-oxygen bond in its molecular chain has a large polarity and has high thermal stability. The Si-O-Si bond protective layer in the structure has a protective effect on the internal structure of the molecule, preventing the gas molecules in the base layer from convecting, forming a continuous insulation layer, effectively inhibiting radiation and convection heat transfer, and thus promoting the card protection film to have a good thermal insulation effect.

[0024] The present invention introduces antistatic sodium sulfonate groups into the polyethylene terephthalate base layer through a chemical reaction. The sodium sulfonate silicone copolyester has similar structural units to polyethylene terephthalate, has hygroscopicity and ion conductivity, and its molecular chain runs through the base layer of the card protection film to form a conductive channel, which is not easy to migrate to the polymer surface, thereby making the antistatic performance of the card protection film lasting. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the structure of the wear-resistant and heat-insulating card protection film. DETAILED DESCRIPTION

[0026] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0027] Para-aminobenzoic acid, CAS number is 150-13-0.

[0028] Sodium 3-chloro-2-hydroxypropane sulfonate, CAS number is 126-83-0.

[0029] Dimethyldichlorosilane, CAS number is 75-78-5.

[0030] Example 1

[0031] (1) Add 66 mL of N,N-dimethylformamide and 30 mmol of p-aminobenzoic acid to a reaction flask, stir evenly, add 27 mmol of sodium 3-chloro-2-hydroxypropane sulfonate and 60 mmol of cesium carbonate, react at 145° C. for 80 h, concentrate under reduced pressure, recrystallize in a 60% volume fraction ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate. The preparation process is as follows:

[0032]

[0033] (2) Add 50 mmol of dimethyldichlorosilane and 90 mL of toluene to the reaction flask, stir evenly, add 110 mmol of 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate sodium and 120 mmol of triethylamine, react at 65° C. for 5 h, concentrate under reduced pressure, recrystallize in 80% ethanol aqueous solution, and dry to obtain sodium dicarboxylate sulfonate organosilicon monomer. The preparation process is as follows:

[0034]

[0035] (3) Add 0.92mmol terephthalic acid, 0.08mmol sodium dicarboxylate sulfonate organosilicon monomer, 1.8mmol ethylene glycol and 0.002mmol tetrabutyl titanate to the reaction flask, stir evenly at 240°C under nitrogen atmosphere, heat to 260°C for polycondensation reaction, the reaction time is 6h, cool and discharge, and obtain sodium sulfonate organosilicon copolyester. The preparation process principle is as follows:

[0036]

[0037] (4) After drying 100 g of polyethylene terephthalate and 8 g of sodium sulfonate silicone copolyester in a vacuum drying oven at a temperature of 125° C. for 16 h, they were added to a high-speed mixer, and then 0.3 g of antioxidant 1010 was added and stirred evenly. The mixture was then melt-extruded on a twin-screw extruder and pelletized by water cooling. The temperatures of the barrel sections of the twin-screw extruder were 300° C., 305° C., 310° C., and 300° C., respectively, and the screw speed was 80 r / min, to obtain modified polyethylene terephthalate.

[0038] (5) After the modified polyethylene terephthalate is melted, it is biaxially stretched at 85°C to obtain a polyester film layer. After being treated with a corona machine, the polyethylene is melted at 200°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted at 205°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 60 r / min and a pulling speed of 8 m / s to obtain a wear-resistant and heat-insulating card protection film.

[0039] Example 2

[0040] (1) Add 160 mL of N,N-dimethylformamide and 80 mmol of p-aminobenzoic acid to a reaction flask, stir evenly, then add 68 mmol of sodium 3-chloro-2-hydroxypropane sulfonate and 120 mmol of cesium carbonate, react at 150° C. for 5 h, concentrate under reduced pressure, recrystallize in a 60% by volume ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate.

[0041] (2) Add 50 mmol of dimethyldichlorosilane and 75 mL of toluene to a reaction flask, stir evenly, then add 102.5 mmol of sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate and 110 mmol of triethylamine, react at 70° C. for 2 h, concentrate under reduced pressure, recrystallize in an ethanol aqueous solution with a volume fraction of 80%, and dry to obtain a sodium dicarboxylic acid sulfonate organosilicon monomer.

[0042] (3) 0.86 mmol of terephthalic acid, 0.14 mmol of sodium dicarboxylate sulfonate organosilicon monomer, 1.6 mmol of ethylene glycol and 0.0015 mmol of tetrabutyl titanate were added to a reaction flask. The mixture was stirred evenly at 250° C. under a nitrogen atmosphere, and then the temperature was raised to 270° C. for polycondensation reaction. The reaction time was 2 h, and the material was cooled and discharged to obtain sodium sulfonate organosilicon copolyester.

[0043] (4) After drying 100 g of polyethylene terephthalate and 13 g of sodium sulfonate silicone copolyester in a vacuum drying oven at 130° C. for 12 h, the mixture was added to a high-speed mixer, and then 0.4 g of antioxidant 1010 was added and stirred evenly. The mixture was then melt-extruded on a twin-screw extruder and pelletized with water cooling. The temperatures of the barrel sections of the twin-screw extruder were 280° C., 305° C., 325° C., and 310° C., respectively, and the screw speed was 60 r / min, to obtain modified polyethylene terephthalate.

[0044] (5) After the modified polyethylene terephthalate is melted, it is biaxially stretched at 80°C to obtain a polyester film layer. After being treated with a corona machine, the polyethylene is melted at 220°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted at 210°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 40 r / min and a pulling speed of 10 m / s to obtain a wear-resistant and heat-insulating card protection film.

[0045] Example 3

[0046] (1) Add 25 mL of N,N-dimethylformamide and 10 mmol of p-aminobenzoic acid to a reaction flask, stir evenly, then add 10 mmol of sodium 3-chloro-2-hydroxypropane sulfonate and 25 mmol of cesium carbonate, react at 130° C. for 10 h, concentrate under reduced pressure, recrystallize in a 60% by volume ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate.

[0047] (2) Add 8 mmol of dimethyldichlorosilane and 16 mL of toluene to a reaction flask, stir evenly, then add 18.4 mmol of sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate and 28 mmol of triethylamine, react at 55° C. for 6 h, concentrate under reduced pressure, recrystallize in an ethanol aqueous solution with a volume fraction of 80%, and dry to obtain a sodium dicarboxylic acid sulfonate organosilicon monomer.

[0048] (3) Add 0.8 mmol of terephthalic acid, 0.2 mmol of sodium dicarboxylate sulfonate organosilicon monomer, 2.0 mmol of ethylene glycol and 0.003 mmol of tetrabutyl titanate into a reaction flask, stir evenly at 220° C. under a nitrogen atmosphere, heat to 255° C. for polycondensation reaction, react for 7 h, cool and discharge to obtain sodium sulfonate organosilicon copolyester.

[0049] (4) After drying 100 g of polyethylene terephthalate and 17 g of sodium sulfonate silicone copolyester in a vacuum drying oven at a temperature of 110° C. for 24 h, they were added to a high-speed mixer, and then 0.5 g of antioxidant 1010 was added and stirred evenly. The mixture was then melt-extruded on a twin-screw extruder and pelletized by water cooling. The temperatures of the barrel sections of the twin-screw extruder were 300° C., 320° C., 325° C., and 310° C., respectively, and the screw speed was 100 r / min, to obtain modified polyethylene terephthalate.

[0050] (5) After the modified polyethylene terephthalate is melted, it is biaxially stretched at 90°C to obtain a polyester film layer. After being treated with a corona machine, the polyethylene is melted at 220°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted at 210°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 80 r / min and a pulling speed of 5 m / s to obtain a wear-resistant and heat-insulating card protection film.

[0051] Example 4

[0052] (1) Add 11.5 mL of N,N-dimethylformamide and 5 mmol of p-aminobenzoic acid to a reaction flask, stir evenly, then add 4.75 mmol of sodium 3-chloro-2-hydroxypropane sulfonate and 12 mmol of cesium carbonate, react at 145° C. for 9 h, concentrate under reduced pressure, recrystallize in a 60% by volume ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate.

[0053] (2) Add 25 mmol of dimethyldichlorosilane and 48 mL of toluene to a reaction flask, stir evenly, then add 56 mmol of sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate and 85 mmol of triethylamine, react at 60° C. for 4 h, concentrate under reduced pressure, recrystallize in an ethanol aqueous solution with a volume fraction of 80%, and dry to obtain a sodium dicarboxylic acid sulfonate organosilicon monomer.

[0054] (3) Add 0.75 mmol of terephthalic acid, 0.25 mmol of sodium dicarboxylate sulfonate organosilicon monomer, 1.9 mmol of ethylene glycol and 0.0025 mmol of tetrabutyl titanate into a reaction flask, stir evenly at 235° C. under a nitrogen atmosphere, raise the temperature to 260° C. for polycondensation reaction, the reaction time is 4 h, and cool the material to obtain sodium sulfonate organosilicon copolyester.

[0055] (4) After drying 100 g of polyethylene terephthalate and 21 g of sodium sulfonate silicone copolyester in a vacuum drying oven at a temperature of 115° C. for 18 h, the mixture was added to a high-speed mixer, and then 0.2 g of antioxidant 1010 was added and stirred evenly. The mixture was then melt-extruded on a twin-screw extruder and pelletized with water cooling. The temperatures of the barrel sections of the twin-screw extruder were 290° C., 310° C., 320° C., and 300° C., respectively, and the screw speed was 85 r / min, to obtain modified polyethylene terephthalate.

[0056] (5) After the modified polyethylene terephthalate is melted, it is biaxially stretched at 80°C to obtain a polyester film layer. After being treated with a corona machine, the polyethylene is melted at 195°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted at 180°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 70 r / min and a pulling speed of 9 m / s to obtain a wear-resistant and heat-insulating card protection film.

[0057] Example 5

[0058] (1) Add 33 mL of N,N-dimethylformamide and 15 mmol of p-aminobenzoic acid to a reaction flask, stir evenly, then add 13.5 mmol of sodium 3-chloro-2-hydroxypropane sulfonate and 30 mmol of cesium carbonate, react at 135° C. for 7 h, concentrate under reduced pressure, recrystallize in a 60% by volume ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate.

[0059] (2) Add 100 mmol of dimethyldichlorosilane and 180 mL of toluene to a reaction flask, stir evenly, then add 210 mmol of sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate and 290 mmol of triethylamine, react at 70° C. for 5 h, concentrate under reduced pressure, recrystallize in an ethanol aqueous solution with a volume fraction of 80%, and dry to obtain a sodium dicarboxylic acid sulfonate organosilicon monomer.

[0060] (3) Add 0.7 mmol of terephthalic acid, 0.3 mmol of sodium dicarboxylate sulfonate organosilicon monomer, 2.0 mmol of ethylene glycol and 0.002 mmol of tetrabutyl titanate into a reaction flask, stir evenly at 240° C. under a nitrogen atmosphere, heat to 260° C. for polycondensation reaction, react for 6 h, cool and discharge to obtain sodium sulfonate organosilicon copolyester.

[0061] (4) After drying 100 g of polyethylene terephthalate and 25 g of sodium sulfonate silicone copolyester in a vacuum drying oven at 125° C. for 14 h, they were added to a high-speed mixer, and then 0.5 g of antioxidant 1010 was added and stirred evenly. The mixture was then melt-extruded on a twin-screw extruder and pelletized with water cooling. The temperatures of the barrel sections of the twin-screw extruder were 280° C., 310° C., 315° C., and 310° C., respectively, and the screw speed was 70 r / min, to obtain modified polyethylene terephthalate.

[0062] (5) After the modified polyethylene terephthalate is melted, it is biaxially stretched at 85°C to obtain a polyester film layer. After being treated with a corona machine, the polyethylene is melted at 205°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, the ethylene-vinyl acetate copolymer is melted at 190°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 65 r / min and a pulling speed of 6 m / s to obtain a wear-resistant and heat-insulating card protection film.

[0063] Comparative Example 1

[0064] After polyethylene terephthalate is melted, it is biaxially stretched at 85°C to obtain a polyester film layer. After being corona treated by a corona machine, polyethylene is melted at 200°C, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, ethylene-vinyl acetate copolymer is melted at 205°C, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled, rolled, and wound by an extruder roller with a rotation speed of 60r / min and a traction speed of 8m / s to obtain a card protection film.

[0065] Wear resistance test: Refer to the standard GB / T 17657-2013 to test the wear resistance of the card protection film. The wear value F is calculated according to the following formula: F = (m 1 -m 2 ) / R×100, where F is the wear value (mg / 100r), m 1 is the mass of the specimen before grinding (mg), m 2 is the mass of the specimen after grinding (mg), and R is the wear revolutions (r).

[0066] Thermal conductivity test: A laser thermal conductivity meter was used to test the thermal conductivity of modified polyethylene terephthalate.

[0067] Table 1 Wear resistance and thermal insulation test

[0068] Wear value (mg / 100r) <![CDATA[Thermal conductivity (W·m -1 ·K -1 )]]> Example 1 0.185 0.272 Example 2 0.116 0.268 Example 3 0.035 0.263 Example 4 0.048 0.259 Example 5 0.076 0.253 Comparative Example 1 0.243 0.281

[0069] It can be seen from the test results in the above table that with the increase of the content of sodium dicarboxylic acid sulfonate silicone monomer in the modified polyethylene terephthalate, the content of silicone increases accordingly, and the wear value of the card protection film gradually decreases. Example 4 reaches 0.048 mg / 100r, and the wear resistance is excellent, while the wear value in Comparative Example 1 is 0.243 mg / 100r, and the wear value is relatively large. This is because the modified polyethylene terephthalate base layer has a Si-O-Si structure, and a highly cross-linked interpenetrating network structure similar to silica is formed when melt solidified, which has good wear resistance and is beneficial to improving the adhesion between the surface layers of the card protection film, forming a card protection film base material with excellent wear resistance.

[0070] Generally speaking, the smaller the thermal conductivity of a material, the better its thermal insulation performance. From the test data in the above table, it can be seen that with the increase of the content of sodium dicarboxylic acid sulfonate silicone monomer in the modified polyethylene terephthalate, the content of silicone increases accordingly, and the thermal conductivity of the modified polyethylene terephthalate gradually decreases, which has a significant thermal insulation effect. This is because the sodium dicarboxylic acid sulfonate silicone monomer reacts with ethylene glycol to form a siloxane polymer with a structure similar to that of polyethylene terephthalate. The silicon-oxygen bond in its molecular chain is very polar and has high thermal stability. The Si-O-Si bond protective layer in the structure protects the internal structure of the molecule, preventing the gas molecules in the base layer from convecting, forming a continuous insulation layer, effectively inhibiting radiation and convection heat transfer, and thus making the card protection film have a good thermal insulation effect.

[0071] Antistatic performance test: After cleaning the surface of the card film, dry it for 24 hours, and test the surface resistivity using a high insulation leakage current meter.

[0072] Table 2 Antistatic test

[0073] Surface resistivity (Ω·cm) Example 1 <![CDATA[9.5×10 13 ]]> Example 2 <![CDATA[2.7×10 13 ]]> Example 3 <![CDATA[5.2×10 12 ]]> Example 4 <![CDATA[8.4×10 11 ]]> Example 5 <![CDATA[1.6×10 11 ]]> Comparative Example 1 <![CDATA[1.2×10 14 ]]>

[0074] It can be seen from the test data in the above table that as the content of sodium dicarboxylic acid sulfonate organosilicon monomer in the modified polyethylene terephthalate increases, the content of sodium sulfonate gradually increases, and the surface resistivity of the card protection film decreases rapidly. The surface resistivity of Example 5 is 1.6×10 11 Ω·cm, indicating that the static charge generated on the surface of the card protection film can be quickly leaked, so that the card protection film has excellent antistatic properties. This is because the sodium sulfonate organosilicon copolyester has hygroscopicity and ion conductivity, and has similar structural units to polyethylene terephthalate, so that its molecular chain runs through the base layer of the card protection film to form a conductive channel, which is not easy to migrate to the polymer surface, thereby making the antistatic property of the card protection film lasting; Comparative Example 1 does not contain sodium sulfonate groups, and its surface resistivity is 1.2×10 14 Ω·cm, poor antistatic performance.

[0075] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A process for preparing a wear-resistant and heat-insulating card protection film, characterized in that: The structure of the card protection film is an ethylene-vinyl acetate copolymer adhesive layer, a polyethylene layer and a modified polyethylene terephthalate base layer from the inner layer to the outer layer, and the preparation process includes the following steps: (1) drying polyethylene terephthalate and sodium sulfonate organosilicon copolyester in a vacuum drying oven at a temperature of 110-130° C. for 12-24 hours, adding the mixture to a high-speed mixer, then adding an antioxidant, stirring the mixture evenly, and then melt-extruding the mixture on a twin-screw extruder, water-cooling and pelletizing the mixture to obtain modified polyethylene terephthalate; (2) After the modified polyethylene terephthalate is melted, it is biaxially stretched to obtain a polyester film layer, and then corona treatment is performed by a corona machine. Then, polyethylene is melted, and a polyethylene film is cast by a casting machine and coated on the polyester film layer. Then, ethylene-vinyl acetate copolymer is melted, and an ethylene-vinyl acetate film is cast by a casting machine and coated on the polyethylene film layer. The film is cooled and rolled by an extruder roller, and then wound and rolled to obtain a wear-resistant and heat-insulating card protection film; The preparation process of the sodium sulfonate organosilicon copolyester comprises the following steps: S1. Add N,N-dimethylformamide and p-aminobenzoic acid to a reaction flask, stir evenly, then add sodium 3-chloro-2-hydroxypropane sulfonate and cesium carbonate, stir to react, and after the reaction is completed, concentrate under reduced pressure, recrystallize in ethanol aqueous solution, and dry to obtain sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate; S2. Add dimethyldichlorosilane and toluene to the reaction flask, stir evenly, add 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate sodium and triethylamine, stir to react, and after the reaction is completed, concentrate under reduced pressure, recrystallize in ethanol aqueous solution, and dry to obtain a molecule with the structural formula: Sodium dicarboxylate sulfonate silicone monomer; S3. Add terephthalic acid, sodium dicarboxylate sulfonate organosilicon monomer, ethylene glycol and tetrabutyl titanate into a reaction flask, stir evenly at 220-250° C. under a nitrogen atmosphere, heat to 255-270° C. for polycondensation reaction, the reaction time is 2-7 hours, cool and discharge to obtain sodium sulfonate organosilicon copolyester.

2. The preparation process of the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In the step (1), the ratio of polyethylene terephthalate, sodium sulfonate organosilicon copolyester and antioxidant is 100g:8-25g:0.1-0.5g.

3. The preparation process of the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In the step (1), the temperatures of the barrel sections of the twin-screw extruder are 280-300°C, 305-320°C, 310-325°C, and 290-310°C, respectively, and the screw speed is 60-100r / min.

4. The preparation process of the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In the step S1, the ratio of p-aminobenzoic acid, N,N-dimethylformamide, sodium 3-chloro-2-hydroxypropane sulfonate and cesium carbonate is 1 mol: 2000-2500 mL: 0.85-1.0 mol: 1.5-2.5 mol.

5. The preparation process of the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In step S1, the reaction temperature is 130-150° C. and the reaction time is 5-10 h.

6. The preparation process of the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In the step S2, the ratio of dimethyldichlorosilane, toluene, sodium 3-((4-carboxyphenyl)amino)-2-hydroxypropane-1-sulfonate, and triethylamine is 1 mol: 1500-2000 mL: 2.05-2.3 mol: 2.2-3.5 mol.

7. The process for preparing the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In step S2, the reaction temperature is 55-70° C. and the reaction time is 2-6 hours.

8. The process for preparing the wear-resistant and heat-insulating card protection film according to claim 1, characterized in that: In the step S3, the ratio of terephthalic acid, sodium dicarboxylic acid sulfonate organic silicon monomer, ethylene glycol, and tetrabutyl titanate is 0.7-0.92 mol: 0.08-0.30 mol: 1.6-2.0 mol: 0.0015-0.003 mol.