A reverse osmosis membrane for efficiently removing small molecule neutral micropollutants and a preparation method thereof
By introducing the CdⅡ/L-cysteine nanowire self-assembly interface into the reverse osmosis membrane and constructing a nano solid-phase intermediate layer, the problem of the existing membrane's poor removal effect of small-molecule neutral micro-pollutants has been solved and achieved A combination of efficient removal and high water permeability.
Patent Information
- Application Number
- CN202410155749.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-04
AI Technical Summary
Existing reverse osmosis membranes are not effective at removing small-molecule neutral micropollutants, and increasing the density of the interception layer will cause loss of water permeability. There is an urgent need to develop membranes with efficient removal capabilities without sacrificing water permeability.
An intermediate layer is introduced between the rejection layer and the base membrane of the reverse osmosis membrane, and CdⅡ/L-cysteine nanowire self-assembly is used to construct a continuous nano solid phase interface. The structure of the rejection layer is controlled through interfacial polymerization to form an excellent small Molecularly neutral micropollutant removal capabilities and high water permeability membrane.
It achieves efficient removal of small-molecule neutral micro-pollutants while maintaining high water permeability, solving the problem of existing membranes’ poor removal effect of small-molecule neutral micro-pollutants, and improving the water permeability of the membrane. .
Smart Images

Figure CN118045495B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane separation, and relates to a reverse osmosis membrane and a preparation method thereof, and in particular to a reverse osmosis membrane for efficiently removing small-molecule neutral micro-pollutants and a preparation method thereof. Background Art
[0002] Micropollutants (such as endocrine disruptors, drugs and antibiotics) are highly toxic and widely present in wastewater. Although they are often present in trace concentrations (ng / L-μg / L), they still pose a significant threat to human health. Therefore, the effective removal of these micropollutants is crucial to ensuring water safety. Reverse osmosis membranes have the advantages of high separation efficiency, good effluent quality, and easy automated control. They are the leading technology for the removal of micropollutants in water. However, the removal effect of existing commercial reverse osmosis membranes for water treatment on small molecule neutral micropollutants (<150Da) is still not ideal.
[0003] Size screening is the main mechanism for the removal of micropollutants by reverse osmosis membranes. In order to achieve efficient removal of small-molecule neutral micropollutants, the retention layer of the reverse osmosis membrane should be dense enough. However, due to the restrictive effect between membrane permeability and selectivity (high solute retention leads to low permeability), simply improving the density of the retention layer of the reverse osmosis membrane will inevitably lead to a loss of membrane water permeability. Therefore, it is urgent to explore effective membrane preparation strategies to develop reverse osmosis membranes with excellent neutral small-molecule micropollutant removal efficiency without sacrificing their water permeability. The introduction of an intermediate layer between the retention layer and the base membrane of the reverse osmosis membrane is expected to regulate the interfacial polymerization reaction process and achieve the regulation of the density of the retention layer of the reverse osmosis membrane. At the same time, the presence of the intermediate layer can also increase the effective water flow area of the retention layer, optimize the water transmission path, and thus improve the water permeability of the reverse osmosis membrane. Therefore, it is urgent to explore a simple, low-cost and efficient intermediate layer introduction strategy. Summary of the invention
[0004] The purpose of the present invention is to provide a reverse osmosis membrane for efficiently removing small molecular neutral micropollutants and a preparation method and application thereof. The present invention adopts amphiphilic Cd Ⅱ / L-cysteine nanowires spontaneously construct a continuous nano-solid phase intermediate layer at the water-oil reaction interface, and in situ regulate the structure of the reverse osmosis membrane retention layer. The membrane has excellent small molecule neutral micro-pollutant removal ability and high water permeability, which is suitable for the efficient removal of small molecule neutral micro-pollutants in water.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a reverse osmosis membrane, the method comprising: first preparing Cd Ⅱ / L-cysteine nanowires, and then formulated with CdⅡ / L-cysteine nanowire n-hexane dispersion, Cd Ⅱ The n-hexane dispersion of L-cysteine nanowires is placed on the surface of the m-phenylenediamine aqueous solution for self-assembly, and then the n-hexane solution of trimesoyl chloride is added to the self-assembly interface to induce an interfacial polymerization reaction, and then deposited on the surface of the base film to form the reverse osmosis membrane.
[0007] In one embodiment of the present invention, the preparation method specifically comprises:
[0008] (1) Preparation of Cd Ⅱ / L-cysteine nanowires: The mixed solution of L-cysteine and Cd(ClO4)2 is adjusted to alkaline, reacted, and after the reaction, solid-liquid separation, washing, and drying are performed to obtain Cd Ⅱ / L-cysteine nanowires;
[0009] (2)Cd Ⅱ / L-cysteine nanowires dispersed in n-hexane solution to obtain Cd Ⅱ / L-cysteine nanowires in n-hexane dispersion were placed on the surface of m-phenylenediamine aqueous solution to self-assemble into continuous Cd Ⅱ / L-cysteine nanowire self-assembly interface;
[0010] (3) Add the trimesoyl chloride n-hexane solution to the Cd Ⅱ / L-cysteine nanowire self-assembly interface, initiating interfacial polymerization to obtain a polyamide retention layer;
[0011] (4) The polyamide retention layer obtained in step (3) and the Cd Ⅱ / L-cysteine nanowires are self-assembled and deposited on the surface of the base membrane to prepare a reverse osmosis membrane.
[0012] In one embodiment of the present invention, in step (1), the mixed solution of L-cysteine and Cd(ClO4)2 can be obtained by directly dissolving L-cysteine and Cd(ClO4)2 in water, or by separately preparing L-cysteine solution and Cd(ClO4)2 solution and then mixing them.
[0013] Furthermore, when L-cysteine solution and Cd(ClO4)2 solution are prepared separately and then mixed, the concentration of L-cysteine in the L-cysteine solution is 0.01-0.1 mol / L, the concentration of Cd(ClO4)2 in the Cd(ClO4)2 solution is 0.004-0.04 mol / L, and the volume ratio of the L-cysteine solution to the Cd(ClO4)2 solution is 1:1.
[0014] In one embodiment of the present invention, in step (1), the pH of the mixed solution after being adjusted to alkaline is 7.5 to 12.0, preferably 7.5 to 8.5.
[0015] In one embodiment of the present invention, in step (1), the adjustment to alkalinity is preferably achieved by adding NaOH solution.
[0016] In one embodiment of the present invention, in step (1), the reaction is preferably carried out at 20-45°C for 48-150h. Under this condition, L-cysteine and Cd(ClO4)2 react and crystallize to obtain Cd Ⅱ / L-cysteine nanowires.
[0017] In one embodiment of the present invention, in step (1), the solid-liquid separation can be performed by centrifugation, filtration or other operation processes known in the art that can separate liquid and solid phases, with the purpose of separating the reaction product from the solvent or unreacted substances; further, the washing is preferably performed by water.
[0018] In one embodiment of the present invention, in step (1), the drying may be vacuum drying or freeze drying; preferably, vacuum drying is performed at 40-80° C. for 8-36 h.
[0019] In one embodiment of the present invention, in step (2), the Cd Ⅱ Cd / L-cysteine nanowires in hexane dispersion Ⅱ The mass fraction of L-cysteine nanowires is 0.01 to 0.2 wt %.
[0020] In one embodiment of the present invention, in step (2), the m-phenylenediamine aqueous solution is an aqueous phase solution, wherein the concentration of m-phenylenediamine is 1.0 to 5.0 wt %.
[0021] In one embodiment of the present invention, in step (2), the self-assembly time is 5 to 15 minutes, and the reaction temperature is 4-35°C, preferably 25°C.
[0022] In one embodiment of the present invention, in step (3), the n-hexane solution of trimesoyl chloride is an oil phase solution, wherein the mass fraction concentration of trimesoyl chloride is 0.05-0.15 wt %.
[0023] In one embodiment of the present invention, in step (3), the interfacial polymerization reaction time is 0.5 to 10 minutes.
[0024] In one embodiment of the present invention, the m-phenylenediamine aqueous solution and the Cd Ⅱ The volume ratio of / L-cysteine nanowire n-hexane dispersion is (40-60):1.
[0025] In one embodiment of the present invention, the volume ratio of the m-phenylenediamine aqueous solution to the trimesoyl chloride n-hexane solution is (15-25):1.
[0026] In one embodiment of the present invention, in step (4), the material of the base membrane can be any one of polysulfone, polyethersulfone, polyimide, polyvinylidene fluoride or polyacrylonitrile, and the molecular weight cutoff of the base membrane is 20-100 kDa.
[0027] The invention also provides a reverse osmosis membrane prepared by the preparation method.
[0028] The invention also provides application of the reverse osmosis membrane in water treatment.
[0029] The beneficial effects of the present invention are:
[0030] 1. The present invention utilizes Cd Ⅱ / The self-assembly characteristics of L-cysteine nanowires construct a continuous nano-solid phase interface at the water-oil interface, promote the pre-enrichment of m-phenylenediamine on the nano-solid phase interface, increase the concentration of m-phenylenediamine in the oil phase, promote interfacial polymerization reaction, and increase the density of the polyamide retention layer of the reverse osmosis membrane, thereby improving the removal efficiency of the reverse osmosis membrane for small molecular neutral micropollutants.
[0031] 2. During the interfacial polymerization reaction, the Cd Ⅱ / L-cysteine nanowire self-assembled nano-solid phase interface can effectively inhibit the dissipation of heat and the escape of nanobubbles, causing the prepared membrane to have a distinct peak-valley structure, increasing the specific surface area of the membrane, and thus improving the water permeability of the reverse osmosis membrane.
[0032] 3. The self-assembled nano-solid phase interface obtained by the present invention can increase the effective water flow area of the interception layer of the reverse osmosis membrane, optimize the water transmission path, reduce the water transmission resistance, and further improve the water permeability of the reverse osmosis membrane.
[0033] 4. The reverse osmosis membrane provided by the present invention has the advantages of simple preparation method, mild conditions, good controllability, low cost, high permeability, good interception effect, etc. It solves the problem that the existing reverse osmosis membrane has poor removal effect on small molecule neutral micro-pollution, and simultaneously improves the water permeability of the membrane, and has a relatively broad application prospect in water treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The present invention will be described in more detail below based on embodiments and with reference to the accompanying drawings, wherein:
[0035] Figure 1 It is a comparison chart of the water permeability of the reverse osmosis membranes prepared in Examples 1 to 3 and Comparative Example 1.
[0036] Figure 2 The scanning electron microscope images of the reverse osmosis membranes prepared in Examples 1 to 3 and Comparative Example 1 are
[0037] Figure 3 It is a comparison chart of the surface area ratio of the reverse osmosis membranes prepared in Examples 1 to 3 and Comparative Example 1.
[0038] Figure 4 It is a comparison chart of the water permeability and NaCl rejection rate of the reverse osmosis membranes prepared in Comparative Examples 3 to 5.
[0039] Figure 5 It is a comparison chart of the retention rates of Example 2 and Comparative Example 1 for 9 nitrogen-containing and chlorine-containing micropollutants with a molecular weight less than 150 Da.
[0040] Figure 6 It is a comparison chart of the water permeability and NaCl retention rate of the membranes prepared in Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] Cd II / Preparation of free interface reverse osmosis membrane regulated by L-cysteine nanowires:
[0044] 1) Add 110 mL of 2.0 wt% m-phenylenediamine aqueous solution into a custom-made container (the container is a cylindrical container with a diameter of 8 cm and a height of 10 cm, the same below) and let it stand until the liquid level is stable.
[0045] 2) Add 2 mL of 0.025 wt% Cd II The hexane suspension of L-cysteine nanowires was evenly dropped onto the surface of the m-phenylenediamine aqueous solution, and a continuous Cd II / L-cysteine nanowire interface; wherein the Cd II / L-cysteine nanowires were prepared by the following method: L-cysteine was dissolved in deionized water to obtain a 0.05 mol / L L-cysteine solution, Cd(ClO4)2·6H2O was dissolved in deionized water to obtain a 0.02 mol / L Cd(ClO4)2 solution, the two were mixed in a volume ratio of 1:1, the pH was adjusted to 8.0 with NaOH, and the mixture was immediately transferred to a constant temperature oven at 37°C for reaction for 120 h, centrifuged and washed with deionized water, and then vacuum dried at 60°C to obtain Cd Ⅱ / L-cysteine nanowires.
[0046] 3) Slowly drop 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution to trigger the interfacial polymerization reaction for 1 min.
[0047] 4) The prepared polyamide retention layer and nanowire interface are deposited onto the surface of a polyethersulfone (PES) based membrane with a molecular weight cutoff of 20,000 Da.
[0048] 5) and rinsed twice with n-hexane solution to obtain RO-0.025 membrane.
[0049] Example 2
[0050] Cd II / Preparation of free interface reverse osmosis membrane regulated by L-cysteine nanowires:
[0051] 1) Add 110 mL of 2.0 wt% m-phenylenediamine aqueous solution into a custom container and let it stand until the liquid level stabilizes.
[0052] 2) Add 2 mL of 0.05 wt% Cd II The n-hexane suspension of L-cysteine nanowires was uniformly dripped onto the surface of the m-phenylenediamine aqueous solution (wherein the Cd II The preparation method of L-cysteine nanowires was the same as that in Example 1), and continuous Cd II / L-cysteine nanowire interface.
[0053] 3) Slowly drop 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution to trigger the interfacial polymerization reaction for 1 min.
[0054] 4) Depositing the prepared polyamide retention layer and nanowire interface onto the surface of a PES-based membrane with a molecular weight cutoff of 20,000 Da.
[0055] 5) and rinsed twice with n-hexane solution to obtain RO-0.05 membrane.
[0056] Example 3
[0057] CdII / Preparation of free interface reverse osmosis membrane regulated by L-cysteine nanowires:
[0058] 1) Add 110 mL of 2.0 wt% m-phenylenediamine aqueous solution into a custom container and let it stand until the liquid level stabilizes.
[0059] 2) Add 2 mL of 0.1 wt% Cd II The n-hexane suspension of L-cysteine nanowires was uniformly dripped onto the surface of the m-phenylenediamine aqueous solution (wherein the Cd II The preparation method of L-cysteine nanowires was the same as that in Example 1), and continuous Cd II / L-cysteine nanowire interface.
[0060] 3) Slowly drop 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution to trigger the interfacial polymerization reaction for 1 min.
[0061] 4) Depositing the prepared polyamide retention layer and nanowire interface onto the surface of a PES-based membrane with a molecular weight cutoff of 20,000 Da.
[0062] 5) and rinsed twice with n-hexane solution to obtain RO-0.1 membrane.
[0063] Comparative Example 1
[0064] No Cd II / Preparation of free interface reverse osmosis membrane regulated by L-cysteine nanowires:
[0065] 1) Add 110 mL of 2.0 wt% m-phenylenediamine aqueous solution into a custom container and let it stand until the liquid level stabilizes.
[0066] 2) Slowly drop 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution to trigger the interfacial polymerization reaction for 1 min.
[0067] 3) The prepared polyamide retention layer is deposited onto the surface of a PES-based membrane with a molecular weight cut-off of 20,000 Da.
[0068] 4) and rinsed twice with n-hexane solution to obtain RO-0 membrane.
[0069] Comparative Example 2
[0070] Preparation of free interface reverse osmosis membrane without pre-enrichment of m-phenylenediamine:
[0071] 1) Add 100 mL of deionized water into a custom container and let it stand until the liquid level stabilizes.
[0072] 2) Add 2 mL of 0.05 wt% CdII / L-cysteine nanowire n-hexane suspension was uniformly dripped on the surface of deionized water (wherein the Cd II The preparation method of L-cysteine nanowires was the same as that in Example 1), and continuous Cd II / L-cysteine nanowire interface.
[0073] 3) 10 mL of a 22 wt % aqueous solution of m-phenylenediamine was added to the above container to make the final concentration of m-phenylenediamine 2.0 wt %.
[0074] 3) Slowly drop 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution to trigger the interfacial polymerization reaction for 1 min.
[0075] 4) Depositing the prepared polyamide retention layer and nanowire interface onto the surface of a PES-based membrane with a molecular weight cutoff of 20,000 Da.
[0076] 5) and rinsed twice with n-hexane solution to obtain NMPD membrane.
[0077] Comparative Example 3
[0078] Preparation of traditional polyamide reverse osmosis membrane:
[0079] 1) A PES ultrafiltration membrane with a molecular weight cutoff of 20,000 Da was used as a porous support layer.
[0080] 2) The PES membrane was placed in a custom-made polytetrafluoroethylene membrane frame, and 5 mL of 2.0 wt % m-phenylenediamine aqueous solution was gently added to the surface of the PES membrane and left for 8 min.
[0081] 3) Then pour out the m-phenylenediamine aqueous solution in the membrane frame and make sure there is no obvious water mark on the surface of the PES membrane.
[0082] 4) Pour 5 mL of a 0.1 wt % hexane solution of trimesoyl chloride onto the surface of the PES membrane saturated with m-phenylenediamine and react for 1 min.
[0083] 5) After the reaction is completed, the trimesoyl chloride n-hexane solution in the membrane frame is poured out, and the membrane frame is rinsed twice with n-hexane solution to obtain a PES-RO membrane.
[0084] Comparative Example 4
[0085] Preparation of traditional polyamide reverse osmosis membrane:
[0086] 1) A PES ultrafiltration membrane with a molecular weight cutoff of 20,000 Da was used as a porous support layer.
[0087] 2) Add 2 mL of 0.05 wt% Cd II / L-cysteine nanowire self-assembled interface loaded onto the PES membrane surface (wherein the Cd II The preparation method of L-cysteine nanowires is the same as that in Example 1) to obtain PES-SAN.
[0088] 3) The PES-SAN membrane was placed in a custom-made polytetrafluoroethylene membrane frame, and 5 mL of 2.0 wt % m-phenylenediamine aqueous solution was gently added to the surface of the PES-SAN membrane and left for 8 min.
[0089] 4) Then pour out the m-phenylenediamine aqueous solution in the membrane frame and make sure there is no obvious water mark on the surface of the PES-SAN membrane.
[0090] 5) Pour 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution onto the surface of the PES-SAN membrane saturated with m-phenylenediamine and react for 1 min.
[0091] 6) After the reaction is completed, the trimesoyl chloride n-hexane solution in the membrane frame is poured out, and the membrane frame is rinsed twice with n-hexane solution to obtain a PES-SAN-RO membrane.
[0092] Comparative Example 5
[0093] Preparation of traditional polyamide reverse osmosis membrane:
[0094] 1) A PES ultrafiltration membrane with a molecular weight cutoff of 20,000 Da was used as a porous support layer.
[0095] 2) Add 2 mL of 0.05 wt% Cd II / L-cysteine nanowires (Cd II The preparation method of L-cysteine nanowires is the same as that of Example 1, without the self-assembly step) and is directly loaded onto the surface of the PES membrane to obtain PES-NSAN.
[0096] 3) The PES-NSAN membrane was placed in a custom-made polytetrafluoroethylene membrane frame, and 5 mL of 2.0 wt % m-phenylenediamine aqueous solution was gently added to the surface of the PES-NSAN membrane and left for 8 min.
[0097] 4) Then pour out the m-phenylenediamine aqueous solution in the membrane frame and make sure there is no obvious water mark on the surface of the PES-NSAN membrane.
[0098] 5) Pour 5 mL of 0.1 wt % trimesoyl chloride n-hexane solution onto the surface of the PES-NSAN membrane saturated with m-phenylenediamine and react for 1 min.
[0099] 6) After the reaction is completed, the trimesoyl chloride n-hexane solution in the membrane frame is poured out, and the membrane frame is rinsed twice with n-hexane solution to obtain a PES-NSAN-RO membrane.
[0100] In order to explore the physicochemical properties and separation performance of the membranes prepared in the embodiments and comparative examples, the present invention provides Experimental Examples 1-3.
[0101] Experimental Example 1
[0102] The membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were tested for pure water permeability. Specifically, the pure water permeability of the prepared reverse osmosis membranes was measured using a cross-flow device under the conditions of 16 bar and 25 ± 0.5 °C. The effective area of the membrane was 6.3 cm 2 The cross flow rate is 20 cm / s, the feed liquid is deionized water, and the volume of water passing through the membrane at a certain time interval is recorded. The pure water permeability is defined as the volume of water passing through a unit membrane area per unit pressure per unit time under certain operating conditions, and its unit is L / (m 2 h bar).
[0103] In addition, the membranes prepared in Example 2 and Comparative Examples 2 to 5 were tested for NaCl retention performance, specifically using a laboratory-scale cross-flow device (the effective area of the membrane pool was 6.3 cm 2 ), pre-press the membrane at 16 bar operating pressure until the membrane flux is stable, the water temperature is 25.0±0.5℃, the cross flow rate is 20 cm / s, the NaCl concentration is 2000 ppm, and the test results are shown in Figure 1 , Figure 4 and Figure 6 .
[0104] Experimental Example 2
[0105] The films prepared in Examples 1 to 3 and Comparative Example 1 were characterized by SEM to visualize their surface morphologies. Figure 2 .
[0106] Experimental Example 3
[0107] The films prepared in Examples 1 to 3 and Comparative Example 1 were subjected to AFM measurement, and the specific surface area of the films (specific surface area = ratio of the actual area of the film to the projected area) was calculated based on the measurement results. The test results are shown in Figure 3 .
[0108] Experimental Example 4
[0109] The reverse osmosis membranes prepared in Example 2 and Comparative Example 1 were tested for micropollutant retention. The concentrations of 9 trace organic pollutants (cis-1,2-dichloroethylene, cis-1,3-dichloropropylene, 1,2-dichloropropane, chloroform, N-nitrosodimethylamine, N-nitrosomethylethylamine, N-nitrosopyrrolidine, N-nitrosodiethylamine, and N-nitrosopiperidine) were all 200 μg / L, and the test conditions were the same as those in Experimental Example 1. The concentrations of nitrogen-containing micropollutants in the inlet and outlet water were determined by high performance liquid chromatography-tandem quadrupole mass spectrometry, while the concentrations of chlorine-containing micropollutants were determined by gas chromatography-tandem mass spectrometry. The test results are shown in Table 1. Figure 5 .
[0110] from Figure 1 It can be seen that the water permeability of the reverse osmosis membranes prepared in Examples 1, 2 and 3 is 2.0±0.3 L·m -2 ·h -1 bar -1 、3.6±0.1L·m -2 ·h -1 bar -1 and 2.7±0.1L·m -2 ·h -1 bar -1 , which is significantly larger than 0.8±0.2L·m in Comparative Example 1 -2 ·h -1 bar -1 This is due to the peak-valley structure of the membrane, which increases its specific surface area and the Cd II / Gully effect at the interface of L-cysteine nanowire self-assembly ( Figure 2 , Figure 3 and Figure 4 ).
[0111] from Figure 5 It can be seen that the reverse osmosis membrane prepared in Example 2 has a significantly improved rejection rate for neutral micropollutants with a molecular weight less than 150 Da, meeting the requirements for wastewater reuse. Figure 6 The results showed that Cd II The pre-enrichment of m-phenylenediamine in the oil phase during the self-assembly process of L-cysteine nanowires is the main reason for the improvement of the membrane pollutant retention rate.
[0112] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for preparing a reverse osmosis membrane, characterized in that: The preparation method specifically comprises: (1) Preparation of Cd Ⅱ / L-cysteine nanowires: The mixed solution of L-cysteine and Cd(ClO4)2 is adjusted to alkaline, reacted, and after the reaction, solid-liquid separation, washing, and drying are performed to obtain Cd Ⅱ / L-cysteine nanowires; (2) Place Cd Ⅱ / L-cysteine nanowires dispersed in n-hexane solution to obtain Cd Ⅱ / L-cysteine nanowires in n-hexane dispersion were placed on the surface of m-phenylenediamine aqueous solution to self-assemble into continuous Cd Ⅱ / L-cysteine nanowire self-assembly interface; (3) Add the hexane solution of trimesoyl chloride to the Cd Ⅱ / L-cysteine nanowire self-assembly interface, initiating interfacial polymerization to obtain a polyamide retention layer; (4) The polyamide retention layer obtained in step (3) and Cd Ⅱ / L-cysteine nanowires are self-assembled and deposited on the surface of the base membrane to prepare a reverse osmosis membrane.
2. The preparation method according to claim 1, characterized in that: In step (1), in step (1), the pH of the mixed solution after being adjusted to alkaline is 7.5-12.
0.
3. The preparation method according to claim 1, characterized in that: In step (1), the reaction is carried out at 20-45°C for 48-150 h.
4. The preparation method according to any one of claims 1 to 3, characterized in that The Cd Ⅱ Cd / L-cysteine nanowires in hexane dispersion Ⅱ / The mass fraction of L-cysteine nanowires is 0.01-0.2 wt %; and / or, the concentration of m-phenylenediamine in the m-phenylenediamine aqueous solution is 1.0-5.0 wt %; and / or, the mass fraction concentration of trimesoyl chloride in the n-hexane solution of trimesoyl chloride is 0.05-0.15 wt %.
5. The preparation method according to claim 4, characterized in that: In step (2), the self-assembly time is 5 to 15 minutes; or, in step (3), the interfacial polymerization reaction time is 0.5 to 10 minutes.
6. The preparation method according to claim 4, characterized in that: The m-phenylenediamine aqueous solution and the Cd Ⅱ The volume ratio of the m-phenylenediamine aqueous solution to the trimesoyl chloride n-hexane solution is (15-25):
1.
7. The preparation method according to any one of claims 1 to 3, 5 to 6, characterized in that: The base film is made of any one of polysulfone, polyethersulfone, polyimide, polyvinylidene fluoride or polyacrylonitrile.
8. The preparation method according to claim 4, characterized in that: The base film is made of any one of polysulfone, polyethersulfone, polyimide, polyvinylidene fluoride or polyacrylonitrile.
9. The reverse osmosis membrane prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the reverse osmosis membrane according to claim 9 in water treatment.
Citation Information
Patent Citations
Preparation method of cadmium telluride / cadmium sulfide core-shell structured nanowires
CN103897701A
Compound nanofiltration membrane with vinylon water-soluble threads as (sacrifice) middle layer and preparing method thereof
CN110404420A
Polyamide film layer composite reverse osmosis membrane as well as preparation method and application thereof
CN112657352A
Polyamide composite membrane with asymmetric double-layer structure as well as preparation method and application of polyamide composite membrane
CN115990411A
Preparation method of polyamide composite nanofiltration membrane containing polystyrene-polyacrylamide nano-microsphere middle layer
CN116672897A