A kind of fully aromatic ester epoxy resin and preparation method thereof
Through the ester bond crosslinking network structure of all aromatic ester epoxy resin, the problem of insufficient thermal conductivity of epoxy resin is solved, and efficient thermal conduction and mechanical performance improvement is achieved, which is suitable for the heat dissipation needs of high-performance electronic devices.
Patent Information
- Application Number
- CN202410090336.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-01-22
AI Technical Summary
The existing epoxy resin has poor thermal conductivity and is difficult to meet the heat dissipation needs of high-performance electronic devices when operating at high frequencies and high power.
Using all-aromatic ester epoxy resin and its preparation method, a uniform and tight crosslinking network is formed during the curing process through the ester bond structure of aromatic ester epoxy monomer and aromatic ester amine curing agent, which improves molecular arrangement and crosslinking structure to form Efficient heat conduction channels and enable regulating molecular structure.
It significantly improves the thermal conductivity of epoxy resin, is suitable for heat dissipation of high-performance electronic devices, and enhances the thermal stability and mechanical properties of the material.
Smart Images

Figure CN118047934B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin preparation, in particular to a fully aromatic ester epoxy resin and a preparation method thereof. Background Art
[0002] Since epoxy resin itself has low thermal conductivity, researchers usually improve its thermal conductivity by adding high thermal conductivity fillers and optimizing the molecular structure of epoxy resin. Adding high thermal conductivity fillers is a common method to enhance the thermal conductivity of epoxy resin. On the one hand, thermal conductive fillers such as metal particles, ceramic particles, and carbon nanotubes usually have excellent thermal conductivity. Adding these fillers to epoxy resin can effectively increase the heat conduction path, thereby significantly improving the thermal conductivity of the material. On the other hand, the type of filler can be controlled to meet the needs of different applications, which is flexible.
[0003] However, this method also has certain limitations. Interfacial thermal resistance is usually formed between the filler and the epoxy matrix, which limits the flow of heat conduction. Good filler dispersion is the key to ensuring that the material has uniform thermal conductivity, but the filler is often not evenly dispersed in the matrix, thus limiting the improvement of thermal conductivity. When the filler content is added at a low level, a complete thermal conductivity path cannot be formed in the matrix, but as the filler content increases, the material's processing performance will deteriorate, and the mechanical properties of the epoxy resin will also be reduced.
[0004] Optimizing the molecular structure of epoxy resin is also an important method to improve its thermal conductivity. Researchers usually introduce liquid crystal units into the epoxy resin system to improve the regularity of molecular arrangement and reduce phonon scattering, thereby improving the intrinsic thermal conductivity of epoxy resin. However, this method usually cannot significantly improve the thermal conductivity of the resin.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a wholly aromatic ester epoxy resin and a preparation method thereof, aiming to solve the problems of poor thermal conductivity of the existing epoxy resin.
[0007] The technical solution of the present invention is as follows:
[0008] A method for preparing a fully aromatic ester epoxy resin comprises the steps of:
[0009] Provide aromatic ester epoxy monomers and aromatic ester amine curing agents;
[0010] The aromatic ester epoxy monomer and the aromatic ester amine curing agent are mixed and heated in an oil bath to obtain a mixture;
[0011] The mixture is subjected to a vacuum treatment to remove bubbles, and then subjected to a curing treatment to obtain a fully aromatic ester epoxy resin.
[0012] The method for preparing the fully aromatic ester epoxy resin, wherein the aromatic ester epoxy monomer comprises one of the following:
[0013] Among them, A is selected from One of: R, R' is independently selected from One of them.
[0014] The preparation method of the fully aromatic ester epoxy resin, wherein the aromatic ester amine curing agent comprises one of the following:
[0015] Among them, A is selected from One of, R, R' are independently selected from One of them.
[0016] The method for preparing the wholly aromatic ester epoxy resin, wherein the temperature of the oil bath heating treatment is 90-120°C, and the time of the oil bath heating treatment is 5-10 minutes; and / or the temperature of the vacuum degassing treatment is 2-5°C higher than the temperature of the oil bath heating treatment, and the time of the vacuum degassing treatment is 15-20 minutes.
[0017] The preparation method of the fully aromatic ester epoxy resin, wherein the curing treatment includes a first curing treatment, a second curing treatment and a third curing treatment; the temperature of the first curing treatment is 95-120°C, and the time of the first curing treatment is 1-2h; the temperature of the second curing treatment is 105-150°C, and the time of the second curing treatment is 2-5h; the temperature of the third curing treatment is 110-180°C, and the time of the third curing treatment is 1-2h.
[0018] The method for preparing the fully aromatic ester epoxy resin, wherein the method for preparing the aromatic ester epoxy monomer comprises the steps of:
[0019] The first monomer, the second monomer, 4-dimethylaminopyridine, N,N'-dicyclohexylcarbodiimide and the first solvent are mixed and reacted to obtain a first intermediate product;
[0020] The first intermediate product is mixed with palladium carbon, palladium hydroxide, and a first solvent, and reduced with hydrogen to obtain a hydroxyl-terminated product;
[0021] The terminal hydroxyl product is dissolved in epichlorohydrin and isopropanol, and sodium hydroxide is added to react, and then washed, precipitated and filtered to obtain an aromatic ester epoxy monomer;
[0022] Wherein, the first monomer is The second monomer is BnO·R1·OH or HO·R1·OH, and R1 is selected from One of them.
[0023] The method for preparing the fully aromatic ester epoxy resin, wherein the molar ratio of the first monomer, the second monomer, the 4-dimethylaminopyridine and the N,N'-dicyclohexylcarbodiimide is (1.05-1.1):1:(1.05-1.1):(1.05-1.1); and / or the total addition amount of the palladium carbon and the palladium hydroxide is 5%-15% of the mass of the second monomer; and / or the molar ratio of the sodium hydroxide to the terminal hydroxyl product is 2:1.
[0024] The preparation method of the fully aromatic ester epoxy resin, wherein the preparation method of the aromatic ester amine curing agent comprises the steps of:
[0025] The third monomer, the fourth monomer, the first solvent and triethylamine are mixed and reacted to obtain a second intermediate product;
[0026] The second intermediate product is mixed with palladium carbon and the first solvent, reduced by hydrogen, and washed and filtered to obtain an aromatic ester amine curing agent;
[0027] Wherein, the third monomer is O2N·R2·COCl, and R2 is selected from The fourth monomer is BnO·R3·OH or HO·R3·OH, R3 is selected from One of them.
[0028] The method for preparing the wholly aromatic ester epoxy resin, wherein the molar ratio of the third monomer, the fourth monomer and the triethylamine is (1.05-1.1):1:(1.05-1.1); and / or the amount of palladium carbon added is 5%-15% of the mass of the fourth monomer.
[0029] A fully aromatic ester epoxy resin is prepared by utilizing the preparation method of the fully aromatic ester epoxy resin.
[0030] Beneficial effects: The present invention provides a fully aromatic ester epoxy resin and a preparation method thereof. The preparation method of the fully aromatic ester epoxy resin comprises the following steps: providing an aromatic ester epoxy monomer and an aromatic ester amine curing agent; mixing the aromatic ester epoxy monomer and the aromatic ester amine curing agent, and subjecting the mixture to oil bath heating treatment to obtain a mixture; subjecting the mixture to vacuum degassing treatment, and then subjecting the mixture to curing reaction to obtain the fully aromatic ester epoxy resin. The present invention utilizes the ester bond structure in both the aromatic ester epoxy monomer and the aromatic ester amine curing agent, so that a stronger chemical interaction can be generated between the two, and a more uniform and more compact cross-linked network structure can be achieved during the curing process. Moreover, the ester bond structure in the epoxy monomer and the curing agent can produce a synergistic effect, further improving the molecular arrangement and the cross-linked structure. This synergistic effect can form a more efficient heat conduction channel. Furthermore, a wider range of molecular structure regulation can be achieved, and not only the number and position of the ester bond can be adjusted in the epoxy molecule, but also similar regulation can be performed in the curing agent, so that the fully aromatic ester epoxy resin has controllability. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a process flow diagram of a method for preparing a wholly aromatic ester epoxy resin;
[0032] Figure 2 is the NMR spectrum of BB-BnO in Example 1;
[0033] Figure 3 is the NMR spectrum of BEP in Example 1;
[0034] Figure 4 is the NMR spectrum of pm-NO in Example 2;
[0035] Figure 5 is the NMR spectrum of pm-NH in Example 2;
[0036] Figure 6 This is a schematic diagram of the reaction equation for preparing BEP-P0 in Example 3;
[0037] Figure 7 This is a schematic diagram of the reaction equation for preparing BEP-P1 in Example 4;
[0038] Figure 8 This is a schematic diagram of the reaction equation for preparing BEP-M2 in Example 5;
[0039] Fig. 9 Schematic diagram of the reaction equation for preparing BEP-PM in Example 6
[0040] Fig.10 TGA diagrams of BEP-P0, BEP-P1, BEP-M2, and BEP-PM;
[0041] Fig.11 DSC diagrams of BEP-P0, BEP-P1, BEP-M2, and BEP-PM;
[0042] Fig.12 It is the tensile performance diagram of BEP-P0, BEP-P1, BEP-M2 and BEP-PM;
[0043] Fig.13 Infrared images of BEP, P0, and BEP-P0;
[0044] Fig.14 Infrared images of BEP, P1, and BEP-P1;
[0045] Fig.15 Infrared images of BEP, M2, and BEP-M2. DETAILED DESCRIPTION
[0046] The present invention provides a fully aromatic ester epoxy resin and a preparation method thereof. To make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0047] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as herein.
[0048] With the development of science and technology, electronic components are gradually developing towards miniaturization, and their stability and reliability are key issues. As the size of electronic devices continues to shrink and the power density continues to increase, high-power devices generate a lot of heat during operation. If they cannot be effectively conducted and dissipated, the performance and stability will be reduced, and even the device will be damaged. With the development of emerging fields such as artificial intelligence, 5G communications, and electric vehicles, some high-performance electronic devices, such as high-performance processors and power amplifiers, need to operate at higher frequencies and powers, so the demand for high-performance heat dissipation materials is more urgent.
[0049] The molecular structure of epoxy resin contains functional groups, which can react with the curing agent through ring opening to form a cross-linked network structure. This cross-linked structure can give epoxy resin excellent mechanical strength and chemical resistance. The molecular structure of epoxy resin gives it good chemical stability and can resist corrosion from chemical substances such as acids, alkalis and other solvents. At the same time, some high-performance epoxy resins have excellent high temperature resistance and moisture resistance. Therefore, epoxy resin is also used as a packaging material for electronic devices. However, in recent years, with the rapid development of the industry, higher requirements have been placed on the thermal conductivity of epoxy resin. Although epoxy resin has the advantages of good mechanical properties, chemical resistance, insulation, versatility, and controllability, its intrinsic thermal conductivity is poor.
[0050] Based on this, Figure 1 As shown, the present invention provides a method for preparing a wholly aromatic ester epoxy resin, comprising the steps of:
[0051] Step S10: providing an aromatic ester epoxy monomer and an aromatic ester amine curing agent;
[0052] Step S20: mixing the aromatic ester epoxy monomer and the aromatic ester amine curing agent, and heating the mixture in an oil bath to obtain a mixture;
[0053] Step S30: After vacuuming and removing bubbles from the mixture, curing is performed to obtain a wholly aromatic ester epoxy resin.
[0054] In this embodiment, aromatic ester epoxy monomer is used as raw material, the compatibility of ester bond and epoxy group is good, and it is easier to form liquid crystal phase under specific conditions. Ester bond can regulate the order of molecules at the molecular level, thereby improving the intrinsic thermal conductivity of epoxy resin; at the same time, aromatic ester amine curing agent with similar structure to epoxy monomer is used, so that both aromatic ester epoxy monomer and aromatic ester amine curing agent contain ester bond structure, which can produce stronger chemical interaction between the two, and can achieve more uniform and tighter cross-linked network structure during curing. In addition, epoxy monomer and curing agent contain ester bond structure at the same time, which can produce synergistic effect, further improve molecular arrangement and cross-linking structure, and this synergistic effect will form a more efficient heat conduction channel, and further can achieve more extensive molecular structure regulation, not only can adjust the number and position of ester bonds in epoxy molecules, but also can make similar regulation in curing agent, and obtain fully aromatic ester epoxy resin with controllability.
[0055] Specifically, the present invention utilizes a diamine monomer with an aromatic ester structure as a curing agent, and cures it with an aromatic ester epoxy monomer to obtain an epoxy resin with a fully aromatic ester structure; aromatic esters can form a liquid crystal structure under specific conditions, improve the orderliness of the structure, reduce phonon scattering, and thus improve the thermal conductivity of the epoxy resin; and the ester bond is a hydrophobic structure, which can improve the water absorption rate of the epoxy resin to a certain extent.
[0056] In some embodiments, the aromatic ester epoxy monomer comprises one of the following:
[0057]
[0058] Among them, A is selected from One of: R, R' is independently selected from One of the above aromatic ester epoxy monomers contains an aromatic ester structure, which can form an orderly arrangement structure and is an epoxy resin containing an ester bond.
[0059] In some embodiments, the aromatic ester amine curing agent is a curing agent containing two amino groups.
[0060] In some embodiments, the aromatic ester amine curing agent includes one of the following:
[0061]
[0062] Among them, A is selected from One of, R, R' are independently selected from One of the above aromatic ester amine curing agents all contain ester bonds and are amine curing agents with a structure similar to that of epoxy monomers.
[0063] Specifically, the aromatic ester epoxy monomer and the aromatic ester amine curing agent both contain ester bond structures, which can generate stronger chemical interactions between the two, and can achieve a more uniform and tighter cross-linked network structure during the curing process. In addition, the epoxy monomer and the curing agent both contain ester bond structures, which can produce a synergistic effect, further improve the molecular arrangement and cross-linking structure, and this synergistic effect will form a more efficient heat conduction channel.
[0064] In some embodiments, the temperature of the oil bath heating treatment is 90-120°C, and the time of the oil bath heating treatment is 5-10 minutes; and / or, the temperature of the vacuum degassing treatment is 2-5°C higher than the temperature of the oil bath heating treatment, and the time of the vacuum degassing treatment is 15-20 minutes. The oil bath heating treatment is used to completely melt the aromatic ester epoxy monomer and the aromatic ester amine curing agent and mix them evenly; the vacuum degassing treatment can be used to remove bubbles in the mixture, thereby avoiding defects such as bubbles in the obtained all-aromatic ester epoxy resin.
[0065] In a preferred embodiment, the temperature of the vacuum debubble treatment is 92-122° C., and the time of the vacuum debubble treatment is 15-20 min.
[0066] In some embodiments, in order to ensure complete curing and improve the comprehensive performance of the epoxy resin after curing, the curing treatment includes a first curing treatment, a second curing treatment and a third curing treatment; the temperature of the first curing treatment is 95-120°C, and the time of the first curing treatment is 1-2h; the temperature of the second curing treatment is 105-150°C, and the time of the second curing treatment is 2-5h; the temperature of the third curing treatment is 110-180°C, and the time of the third curing treatment is 1-2h.
[0067] In some embodiments, the vacuum debubbling treatment is performed in a vacuum oven, and the vacuum is drawn 1-3 times to remove bubbles.
[0068] In some embodiments, the molar ratio of the aromatic ester epoxy monomer to the aromatic ester amine curing agent is 2:1, and one epoxy group corresponds to one hydrogen.
[0069] In some embodiments, the method for preparing the aromatic ester epoxy monomer comprises the steps of:
[0070] Step S1: mixing and reacting a first monomer, a second monomer, 4-dimethylaminopyridine, N,N'-dicyclohexylcarbodiimide and a first solvent to obtain a first intermediate product;
[0071] Step S2: mixing the first intermediate product with palladium carbon, palladium hydroxide, and a first solvent, and reducing the mixture with hydrogen to obtain a terminal hydroxyl product;
[0072] Step S3: dissolving the terminal hydroxyl product in epichlorohydrin and isopropanol, adding sodium hydroxide to react, washing, precipitating and filtering to obtain an aromatic ester epoxy monomer;
[0073] Wherein, the first monomer is The second monomer is BnO·R1·OH or HO·R1·OH, and R1 is selected from One of them.
[0074] In this embodiment, the above-mentioned preparation method can be used to introduce an aromatic ester structure into the epoxy monomer to form an effective arrangement structure, thereby obtaining an epoxy resin containing an ester bond; the ester bond has good compatibility with the epoxy group and is more likely to form a liquid crystal phase under specific conditions, and the ester bond can regulate the order of the molecule at the molecular level, thereby improving the intrinsic thermal conductivity of the epoxy resin.
[0075] In some embodiments, the molar ratio of the first monomer, the second monomer, the 4-dimethylaminopyridine and the N,N'-dicyclohexylcarbodiimide is (1.05-1.1):1:(1.05-1.1):(1.05-1.1); and / or the total addition amount of the palladium carbon and the palladium hydroxide is 5%-15% of the mass of the second monomer; and / or the molar ratio of the sodium hydroxide to the terminal hydroxyl product is 2:1.
[0076] In a preferred embodiment, the molar ratio of the first monomer, the second monomer, the 4-dimethylaminopyridine and the N,N'-dicyclohexylcarbodiimide is 1.05:1:1.05:1.05.
[0077] Specifically, the first monomer, the second monomer, 4-dimethylaminopyridine, and N,N'-dicyclohexylcarbodiimide are added to a flat-bottomed flask, and a solvent is added for stirring, and the reaction is carried out for 6-8 hours. After the reaction is completed, the solvent is spin-dried, and washed with ethanol 2-3 times, and filtered to obtain a first intermediate product; the first intermediate product, palladium carbon, and palladium hydroxide are placed in a flat-bottomed flask, tetrahydrofuran, DMF and other solvents are added, hydrogen is introduced, and a reduction reaction is carried out. The reaction time is 24-72 hours. After the reaction is completed, filtering is carried out, and the filtrate is spin-dried to obtain a terminal hydroxyl product; the terminal hydroxyl product, epichlorohydrin, and isopropanol are added Pour into a round-bottom flask, and put into an oil pan at 55-65°C, heat and stir until the terminal hydroxyl product is completely dissolved; then add sodium hydroxide dropwise, react for 2-4h, add an equal amount of sodium hydroxide again, react for 4-8h, and when the reaction is over, take out the flask and wait for it to cool to room temperature; pour the solution after the reaction into a separatory funnel, add water, separate the liquid, take the organic phase, and repeat the operation twice; pour the obtained organic phase into 2-3 times of ethanol, filter if solid precipitates, and the filter residue is the primary product, and add n-hexane or petroleum ether to the primary product, wash 1-2 times, and finally filter to obtain the aromatic ester epoxy monomer.
[0078] In some embodiments, the amount of the first solvent is 6-8 times the mass of the second monomer.
[0079] In some embodiments, the molar ratio of the terminal hydroxyl product to the epichlorohydrin is 1:(10-2), and the amount of isopropanol used is 40-50 wt % of the epichlorohydrin.
[0080] In some embodiments, the method for preparing the aromatic ester amine curing agent comprises the steps of:
[0081] Step SS1: mixing and reacting the third monomer, the fourth monomer, the first solvent and triethylamine to obtain a second intermediate product;
[0082] Step SS2: mixing the second intermediate product with palladium carbon and the first solvent, reducing the mixture with hydrogen, washing and filtering the mixture to obtain an aromatic ester amine curing agent;
[0083] Wherein, the third monomer is O2N·R2·COCl, and R2 is selected from The fourth monomer is BnO·R3·OH or HO·R3·OH, R3 is selected from One of them.
[0084] In this embodiment, an ester bond is introduced into the curing agent to obtain an amine curing agent with a structure similar to that of the epoxy monomer. The simultaneous introduction of the ester bond structure into the epoxy monomer and the curing agent can produce a stronger chemical interaction between the two, and can achieve a more uniform and tighter cross-linked network structure during the curing process. In addition, the epoxy monomer and the curing agent both contain an ester bond structure, which can produce a synergistic effect, further improve the molecular arrangement and cross-linking structure, and this synergistic effect will form a more efficient heat conduction channel.
[0085] In some embodiments, the molar ratio of the third monomer, the fourth monomer and the triethylamine is (1.05-1.1):1:(1.05-1.1); and / or, the added amount of the palladium carbon is 5%-15% of the mass of the fourth monomer.
[0086] In a preferred embodiment, the molar ratio of the third monomer, the fourth monomer and the triethylamine is 1.05:1:1.05.
[0087] In some embodiments, the first solvent is selected from but not limited to one or more of dichloromethane, tetrahydrofuran, and dimethylacetamide.
[0088] Specifically, the third monomer and the fourth monomer are added to a flat-bottomed flask, a first solvent such as dichloromethane, tetrahydrofuran, etc. is added, and triethylamine is added dropwise to the system, stirred, and reacted for 6-8 hours. After the reaction is completed, the solvent is spin-dried, washed with ethanol 2-3 times, and filtered to obtain a second intermediate product; the second intermediate product and palladium carbon are diluted into a flat-bottomed flask, tetrahydrofuran, DMF and other solvents are added, hydrogen is introduced, and a reduction reaction is carried out. The reaction is reacted for 24-72 hours. After the reaction is completed, it is filtered, and the filtrate is dropped into a large amount of water for stirring, and filtered to obtain an aromatic ester amine curing agent.
[0089] In some embodiments, the amount of the first solvent is 6-8 times the mass of the fourth monomer.
[0090] In addition, the present invention also provides a wholly aromatic ester epoxy resin, which is prepared by using the preparation method of the wholly aromatic ester epoxy resin.
[0091] In some embodiments, the application of the wholly aromatic ester epoxy resin in electronic packaging materials has good thermal conductivity, which is beneficial to timely dissipate the heat of electronic devices.
[0092] The following examples are further given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention.
[0093] Example 1
[0094] In this embodiment, a aromatic ester epoxy monomer (BEP) is prepared, and the preparation steps include the following:
[0095] 50g of p-benzyloxyphenol, 60g of p-benzyloxybenzoic acid, 32g of 4-dimethylaminopyridine, and 54.25g of N,N'-dicyclohexylcarbodiimide were added to a single-necked flask containing 500ml of dichloromethane, with a raw material molar ratio of 1:1.05:1.05:1.05, and the reaction was carried out for 8h. After the reaction, the dichloromethane was spin-dried, washed with ethanol for more than 2 times, and dried to obtain the intermediate product BB-BnO. The NMR spectrum of BB-BnO is shown in Figure 2 As shown, BB-BnO was successfully prepared, and its chemical structure is
[0096] The intermediate product BB-BnO was added to a single-necked flask, and 8 times the mass of tetrahydrofuran was added, and a catalyst of 15% palladium carbon and 15% palladium hydroxide was added, and the reaction was carried out by hydrogen reduction for 48 hours. After the reaction was completed, the catalyst was filtered, and BB-OH was obtained by rotary evaporation, washing with ethanol, and drying, indicating that BB-OH was successfully prepared.
[0097] Add BB-OH, epichlorohydrin and isopropanol into a three-necked flask (the molar ratio of BB-OH to epichlorohydrin is 1:20, and the amount of isopropanol added is 45% of the mass of epichlorohydrin), put the flask into a 65°C oil pan, and wait for BB-OH to completely dissolve. Add 10% sodium hydroxide by mass (add an amount equal to the molar ratio of BB-OH) dropwise, react for 3 hours, add the same amount of sodium hydroxide again, and react for 4 hours. After the reaction is completed, cool to room temperature, wash with water 3 times, take the organic phase, add the organic phase to ethanol, a precipitate is precipitated, filter to obtain the precipitate, add the precipitate to n-hexane for washing, and finally filter to obtain the aromatic ester epoxy monomer (BEP). The NMR spectrum of BEP is shown as follows Figure 3 shown.
[0098] Example 2
[0099] In this embodiment, an aromatic ester amine curing agent (pm-NH) is prepared, and the preparation steps include the following:
[0100] Weigh p-nitrophenol, m-nitrobenzoyl chloride, and triethylamine (molar ratio of 1:1.05:1.05), first add nitrophenol and m-nitrobenzoyl chloride into a flat-bottom flask, add 8 times of dichloromethane, and drop triethylamine into the system for 8 hours of reaction. After the reaction is completed, spin-dry the dichloromethane, wash it with ethanol 1-2 times, and dry it to obtain the product pm-NO. The NMR spectrum of pm-NO is as follows: Figure 4 As shown, it shows that pm-NO was successfully prepared, and its chemical structure is
[0101] The product pm-NO was placed in a flat-bottomed flask, 8 times DMF was added, 10% mass fraction of palladium carbon was added, and hydrogen was used for reduction. The reaction was continued for 48 hours. After the reaction was completed, the palladium carbon was filtered. The filtrate was dripped into water and filtered to obtain the product, which was washed with ethanol, filtered, and dried to obtain an aromatic ester amine curing agent (pm-NH). The NMR spectrum of pm-NH is shown as follows: Figure 5 As shown, it shows that pm-NO was successfully prepared, and its chemical structure is
[0102] Example 3
[0103] This embodiment uses As raw material, prepare whole aromatic ester epoxy resin (BEP-P0), comprising the following steps:
[0104] Preparation of BEP-P0: Prepare an oil bath at 90°C and an oven at 95°C in advance and preheat the silicone mold in the oven. Weigh 7g of epoxy monomer BEP and 1.106g of P0 and add them to a single-necked flask with a magnet. Heat the flask in an oil bath. Add 0.5ml of DMF solution in batches during the heating process, and wait for the mixture to completely melt into a liquid with a certain fluidity. Take the flask out of the oil bath and quickly transfer it to the oven. Pay attention to heat preservation during the transfer. Pour the liquid into molds of different sizes and vacuum them. The vacuuming time is within 20min. The effect of removing bubbles is achieved by multiple vacuuming methods. After removing bubbles, cure with a curing program of 95°C for 2h, 105°C for 2h, and 120°C for 1h. After complete curing, wait for the oven to cool down naturally to room temperature, take out the silicone mold, and obtain a cured epoxy resin.
[0105] The reaction equation of this embodiment is as follows Figure 6 shown.
[0106] Example 4
[0107] This embodiment uses As raw materials, a fully aromatic ester epoxy resin (BEP-P1) is prepared, comprising the following steps:
[0108] Preparation of BEP-P1: Prepare an oil bath at 120°C and an oven at 122°C in advance and preheat the silicone mold in the oven. Weigh 10g of epoxy monomer BEP and 3.333g of P1 and add them to a single-necked flask with a magnet. Heat the flask in an oil bath. Add 0.5ml of DMF solution in batches during the heating process and wait for the mixture to completely melt into a liquid with a certain fluidity. Take the flask out of the oil bath and quickly transfer it to the oven. Pay attention to heat preservation during the transfer. Pour the liquid into molds of different sizes and vacuum them. The vacuuming time is within 20 minutes. The effect of removing bubbles is achieved by vacuuming multiple times. After removing bubbles, cure with a curing program of 122°C for 2h, 150°C for 2h, and 180°C for 1h. After complete curing, wait for the oven to cool down naturally to room temperature, take out the silicone mold, and obtain a cured epoxy resin.
[0109] The reaction equation of this embodiment is as follows Figure 7 shown.
[0110] Example 5
[0111] This embodiment uses As raw materials, a fully aromatic ester epoxy resin (BEP-M2) is prepared, comprising the following steps:
[0112] Preparation of BEP-M2: Prepare an oil bath at 120°C and an oven at 122°C in advance and preheat the silicone mold in the oven. Weigh 5g of epoxy monomer BEP and 2.546g of M2 and add them to a single-necked flask with a magnet. Place the flask in an oil bath and heat it. Add 0.5ml of DMF solution in batches during the heating process and wait for the mixture to completely melt into a liquid with a certain fluidity. Take the flask out of the oil bath and quickly transfer it to the oven. Pay attention to heat preservation during the transfer. Pour the liquid into molds of different sizes and vacuum them. The vacuuming time is within 20 minutes. The effect of removing bubbles is achieved by vacuuming multiple times. After removing bubbles, cure with a curing program of 122°C for 2h, 150°C for 2h, and 180°C for 1h. After complete curing, wait for the oven to cool down naturally to room temperature, take out the silicone mold, and obtain a cured epoxy resin.
[0113] The reaction equation of this embodiment is as follows Figure 8 shown.
[0114] Example 6
[0115] This embodiment uses As raw materials, preparing a fully aromatic ester epoxy resin (BEP-PM) comprises the following steps:
[0116] Preparation of BEP-PM: Prepare an oil bath at 120°C and an oven at 122°C in advance and preheat the silicone mold in the oven. Weigh 10g of epoxy monomer BEP and 3.333g of PM and add them to a single-necked flask with a magnet. Heat the flask in an oil bath. Add 0.5ml of DMF solution in batches during the heating process and wait for the mixture to completely melt into a liquid with a certain fluidity. Take the flask out of the oil bath and quickly transfer it to the oven. Pay attention to heat preservation during the transfer. Pour the liquid into molds of different sizes and vacuum them. The vacuuming time is within 20 minutes. The effect of removing bubbles is achieved by vacuuming multiple times. After removing bubbles, cure with a curing program of 115°C for 2h, 145°C for 2h, and 175°C for 2h. After complete curing, wait for the oven to cool down naturally to room temperature, take out the silicone mold, and obtain a cured epoxy resin.
[0117] The reaction equation of this embodiment is as follows Fig. 9 shown.
[0118] The performance tests of BEP-P0, BEP-P1, BEP-M2 and BEP-PM prepared in Examples 3 to 6 were carried out, and their TGA graphs, DSC graphs and tensile performance graphs were shown as follows: Fig.10 , Fig.11 , Fig.12 As shown; In addition, the infrared images of BEP-P0, BEP-P1, and BEP-M2 are shown as follows Fig.13 , Fig.14 and Fig.15 As shown, the five regions from left to right in the figure are -NH2 absorption peak, ester bond carbonyl stretching vibration peak, benzene ring skeleton stretching vibration, ether bond -CO absorption peak and epoxy group absorption peak.
[0119] from Fig.10 It can be seen that the temperatures at which P0, P1, M2 and PM lose 5% of their weight are 333°C, 370°C, 389°C and 320°C respectively, indicating that the epoxy resin prepared in the present invention has good thermal stability; Fig.11 It can be seen that the glass transition temperature of the epoxy resin prepared in the present invention is above 100°C, and has good heat resistance; Fig.12 It can be seen that the epoxy resin prepared in the present invention has good tensile strength.
[0120] In summary, the present invention provides a fully aromatic ester epoxy resin and a preparation method thereof, and the preparation method of the fully aromatic ester epoxy resin comprises the steps of: providing an aromatic ester epoxy monomer and an aromatic ester amine curing agent; mixing the aromatic ester epoxy monomer and the aromatic ester amine curing agent, and heating the mixture in an oil bath to obtain a mixture; vacuumizing and removing bubbles from the mixture, and then performing a curing reaction to obtain a fully aromatic ester epoxy resin. The present invention utilizes the ester bond structure in both the epoxy molecule and the curing agent to produce a stronger chemical interaction between the two, and can achieve a more uniform and more compact cross-linked network structure during the curing process. In addition, the ester bond in the epoxy monomer and the curing agent will produce a synergistic effect, further improving the molecular arrangement and cross-linking structure, and this synergistic effect will form a more efficient heat conduction channel; further, it can achieve a wider range of molecular structure regulation, not only can the number and position of the ester bond be adjusted in the epoxy molecule, but also similar regulation can be performed in the curing agent, so that the fully aromatic ester epoxy resin has controllability.
[0121] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a wholly aromatic ester epoxy resin, characterized in that: Includes steps: Provide aromatic ester epoxy monomers and aromatic ester amine curing agents; The aromatic ester epoxy monomer and the aromatic ester amine curing agent are mixed and heated in an oil bath to obtain a mixture; The mixture is subjected to a vacuum treatment to remove bubbles, and then subjected to a curing treatment to obtain a fully aromatic ester epoxy resin; The aromatic ester epoxy monomer comprises one of the following: , , , , , , , ; The aromatic ester amine curing agent comprises one of the following: , , , , , , , , ; Among them, A is selected from , One of, R, R' are independently selected from , , , , One of; The temperature of the oil bath heating treatment is 90-120°C, and the time of the oil bath heating treatment is 5-10 minutes; and / or the temperature of the vacuum degassing treatment is 2-5°C higher than the temperature of the oil bath heating treatment, and the time of the vacuum degassing treatment is 15-20 minutes; the vacuum degassing treatment is carried out in a vacuum oven, and the air bubbles are removed by vacuuming 1-3 times; the molar ratio of the aromatic ester epoxy monomer to the aromatic ester amine curing agent is 2:1; The curing treatment includes sequentially performing a first curing treatment, a second curing treatment and a third curing treatment; the temperature of the first curing treatment is 95-120°C, and the time of the first curing treatment is 1-2 hours; the temperature of the second curing treatment is 105-150°C, and the time of the second curing treatment is 2-5 hours; the temperature of the third curing treatment is 110-180°C, and the time of the third curing treatment is 1-2 hours; The method for preparing the aromatic ester epoxy monomer comprises the steps of: The first monomer, the second monomer, 4-dimethylaminopyridine, N,N'-dicyclohexylcarbodiimide and the first solvent are mixed and reacted to obtain a first intermediate product; The first intermediate product is mixed with palladium carbon, palladium hydroxide, and a first solvent, and reduced with hydrogen to obtain a hydroxyl-terminated product; The terminal hydroxyl product is dissolved in epichlorohydrin and isopropanol, and sodium hydroxide is added to react, and then washed, precipitated and filtered to obtain an aromatic ester epoxy monomer; Wherein, the first monomer is ; The second monomer is BnO·R1·OH or HO·R1·OH, R1 is selected from , , , , One of; The amount of the first solvent is 6-8 times the mass of the second monomer; the molar ratio of the terminal hydroxyl product to the epichlorohydrin is 1:(10-2), and the amount of isopropanol used is 40-50wt% of epichlorohydrin.
2. The method for preparing a wholly aromatic ester epoxy resin according to claim 1, wherein The molar ratio of the first monomer, the second monomer, the 4-dimethylaminopyridine and the N,N'-dicyclohexylcarbodiimide is (1.05-1.1):1:(1.05-1.1):(1.05-1.1); and / or the total added amount of the palladium carbon and the palladium hydroxide is 5%-15% of the mass of the second monomer; and / or the molar ratio of the sodium hydroxide to the terminal hydroxyl product is 2:
1.
3. The method for preparing a wholly aromatic ester epoxy resin according to claim 1, wherein The preparation method of the aromatic ester amine curing agent comprises the steps of: The third monomer, the fourth monomer, the first solvent and triethylamine are mixed and reacted to obtain a second intermediate product; The second intermediate product is mixed with palladium carbon and the first solvent, reduced by hydrogen, and washed and filtered to obtain an aromatic ester amine curing agent; Wherein, the third monomer is O2N·R2·COCl, and R2 is selected from , , The fourth monomer is BnO·R3·OH or HO·R3·OH, R3 is selected from , , , , One of them.
4. The method for preparing a wholly aromatic ester epoxy resin according to claim 3, wherein: The molar ratio of the third monomer, the fourth monomer and the triethylamine is (1.05-1.1):1:(1.05-1.1); and / or, the added amount of the palladium carbon is 5%-15% of the mass of the fourth monomer.
5. A fully aromatic ester epoxy resin, characterized in that: The invention is prepared by the preparation method of the wholly aromatic ester epoxy resin as described in any one of claims 1 to 4.
Citation Information
Cited By
Liquid crystal curing agent, preparation method thereof and application of liquid crystal curing agent in intrinsic high-thermal-conductivity polymer curing
CN121085792A