Application of nickel-iron-lanthanum ternary supported catalyst in microwave-driven steam reforming of low-carbon alcohols to produce hydrogen
The problem of easy carbon deposit and high by-product selectivity of catalysts in hydrogen reforming of ethanol water vapor is solved by using graphitized carbon nanotubes and molybdenum carbide under microwave drive, and high efficiency is achieved low-temperature and high-efficiency hydrogen production and low-cost hydrogen production.
Patent Information
- Application Number
- CN202410208339.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-26
AI Technical Summary
In the existing ethanol water vapor reforming hydrogen production technology, the catalyst is prone to carbon accumulation and high selectivity of by-products, resulting in low hydrogen production efficiency, and the reaction temperature of the traditional heating process is high, making it difficult to reduce.
Under microwave-driven use of graphitized carbon nanotubes and molybdenum carbide as support and additives to improve the activity and conductivity of the catalyst, reduce the reaction temperature and enhance the energy utilization rate.
Under microwave reaction conditions of 470°C and below, the H2 yield of ethanol reached 4.91 mol/mol, the alcohol conversion rate exceeded 90%, and the selectivity of by-products CH4 and CO was reduced, achieving efficient utilization of low-carbon mixed alcohols, reducing Cost and energy loss of hydrogen production process.
Smart Images

Figure CN118062807B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microwave-driven ethanol steam reforming hydrogen production, and in particular to the application of a nickel-iron-lanthanum ternary supported catalyst in microwave-driven low-carbon alcohol steam reforming hydrogen production reaction. Background Art
[0002] The alcohol / steam reforming hydrogen production method represented by low-carbon alcohols such as ethanol and methanol has great value in small-scale and decentralized hydrogen use scenarios due to its flexible use. The alcohol-hydrogen route is conducive to overcoming the difficulties in hydrogen storage and transportation. As a liquid hydrogen carrier, ethanol has the advantages of high energy density, low toxicity and easy storage and transportation, and is an ideal raw material for steam reforming hydrogen production. Especially when bioethanol derived from biomass is used as a raw material, ethanol steam reforming technology is an important bridge between renewable energy and net zero emission hydrogen production processes. In addition, in typical chemical processes such as Fischer-Tropsch synthesis or pharmaceuticals, which use low-carbon alcohols as solvents, there are often waste solutions of low-carbon alcohols containing ethanol. For example, the aqueous by-product of Fischer-Tropsch synthesis is mainly a mixture of C1-C8 alcohols and water. Usually, C4-C8 mixed alcohols are separated and used as fuel; C1-C3 mixed alcohols can be used as low-value chemical raw materials due to their relatively low calorific value. Low-carbon mixed alcohols mainly C1-C3 are also usually used in the process of synthesizing low-carbon alcohols from syngas. In industrial production, C1-C3 low-carbon alcohols are also often used as solvents. After being discarded, these solvents may be mixed due to poor management or other process reasons. In addition to methanol, ethanol, propanol and isopropanol in C1-C3 low-carbon alcohols all form azeotropes with water, which makes the separation and purification of low-carbon mixed alcohols difficult and costly. If low-carbon mixed alcohols containing ethanol are directly used as raw materials for steam reforming hydrogen production without separation and purification, the source of raw materials for steam reforming hydrogen production will be expanded, which can reduce costs and enhance the sustainability of the hydrogen production process.
[0003] At present, ethanol steam reforming hydrogen production is mainly carried out in a traditional heating process, and the reaction temperature is usually 600-750°C. Reducing the temperature of the ethanol steam reforming hydrogen production process is of great significance to improving the energy efficiency of the hydrogen production process. The literature Advanced Energy Materials, 2023, 13(48): 202301920 constructed a series of Mo 2 TiC 2TxMxene-loaded Ni catalyst is used for steam reforming of bioethanol to produce hydrogen at low temperature. When the Ni content is 10%, the reforming reaction effect is the best, and the reaction temperature is still as high as 550°C. Compared with methanol, ethanol molecules have CC bonds, and the reaction path of its steam reforming is more complicated than that of methanol steam reforming. The catalyst for ethanol steam reforming should have a strong ability to catalyze CC bond breaking. As a low-cost non-precious metal, Ni-based catalysts have strong CC bond breaking ability and high activity for methane reforming and CO shift reactions. They are commonly used basic catalysts in ethanol steam reforming reactions; however, Ni-based catalysts are prone to carbon deposition and are sensitive to CO and CO at low temperatures. 2 The methanogenic activity of these catalysts is stronger than their reforming activity for methane, and they usually have problems such as high selectivity for methane by-products and low hydrogen production efficiency due to carbon deposition and deactivation. Summary of the invention
[0004] The purpose of the present invention is to provide an application of a nickel-iron-lanthanum ternary supported catalyst in a microwave-driven low-carbon alcohol steam reforming hydrogen production reaction, especially in a microwave-driven ethanol or C1-C3 mixed alcohol containing ethanol and steam reforming hydrogen production reaction. The nickel-iron-lanthanum ternary supported catalyst has high activity and high alcohol conversion rate under microwave radiation.
[0005] To achieve the above object, the technical scheme adopted by the present invention is as follows: application of nickel-iron-lanthanum ternary supported catalyst in microwave-driven low-carbon alcohol steam reforming hydrogen production reaction, wherein the active component of the nickel-iron-lanthanum ternary metal supported catalyst is Ni-Fe-La, and the carrier is graphitized carbon nanotubes, the carbon content of the carbon nanotubes is ≧99.9%, the tube diameter is 8-15nm, the tube length is 10-50μm, and 0.01≦I D / I G ≦1.0, the auxiliary agent is molybdenum carbide, and the catalyst is composed of the following components in weight percentage: 18-22% nickel oxide, 37-44% iron oxide, 2-11% lanthanum oxide, 22-33% carbon nanotubes, and 11-16.5% molybdenum carbide; the added amount of molybdenum carbide is 0.5-0.75 times the weight of the carbon nanotubes.
[0006] Preferably, the particle size of the molybdenum carbide is 0.01-200 μm.
[0007] Preferably, the preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include: (1) firstly using nickel oxide, iron oxide, and lanthanum oxide precursors as raw materials, grinding and calcining to obtain catalyst active components, and then mechanically grinding with a moderately graphitized carbon nanotube carrier to obtain a Ni-Fe-La / CNTs catalyst; (2) based on the Ni-Fe-La / CNTs catalyst, introducing a molybdenum carbide component, and using a dry ball milling mechanical mixing method or an organic solvent-assisted dispersion method to mix the molybdenum carbide and the Ni-Fe-La / CNTs catalyst to obtain a Ni-Fe-La / CNTs-MoC 2 catalyst.
[0008] Further preferably, the preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include: (1) using water as a solvent, using moderately graphitized carbon nanotubes as a carrier, and using precursors of nickel oxide, iron oxide, and lanthanum oxide as raw materials for impregnation synthesis to obtain a Ni-Fe-La / CNTs supported catalyst; (2) based on the Ni-Fe-La / CNTs supported catalyst, introducing a molybdenum carbide component, and using a dry ball milling mechanical mixing method or an organic solvent-assisted dispersion method to uniformly mix the molybdenum carbide and the Ni-Fe-La / CNTs catalyst to obtain a Ni-Fe-La / CNTs-MoC 2 catalyst.
[0009] Preferably, the precursors of the nickel oxide, iron oxide and lanthanum oxide are one or more of nitrates and hydrates thereof, acetates and hydrates thereof or hydroxides of the corresponding metals.
[0010] More preferably, the precursors of the nickel oxide, iron oxide and lanthanum oxide are nickel acetate hydrate, iron nitrate hydrate and lanthanum nitrate hydrate, respectively.
[0011] More preferably, the preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include:
[0012] S1: According to NiO and Fe 2 O 3 The mass ratio is 0.5-1, La 2 O 3 Precursors of nickel oxide, iron oxide and lanthanum oxide are weighed and mixed respectively, accounting for 3-15% by mass in the active component, and deionized water of 2-5 times the mass of the above mixture is added and stirred and dispersed, and then graphitized carbon nanotubes are added, stirred evenly and ultrasonicated for 2 hours; the mass ratio of graphitized carbon nanotubes to active components is 0.33-1;
[0013] S2: stirring the mixed raw material obtained in step S1 at room temperature for 3 hours to allow the metal active components to be better dispersed and impregnated on the graphitized carbon nanotubes; after 3 hours, stirring and heating are started to evaporate the water until the material becomes a viscous colloidal slurry, and then transferred to an air environment at 100-160°C for further drying;
[0014] S3: Transfer the catalyst precursor obtained in step S2 into an inert atmosphere, raise the temperature to 400-650° C. and maintain for 2-3 hours;
[0015] S4: grinding the catalyst obtained in step S3 into powder with a particle size of 2-500 μm to obtain a Ni-Fe-La / CNTs supported catalyst;
[0016] S5: mixing the Ni-Fe-La / CNTs supported catalyst obtained in step S4 with molybdenum carbide and pre-stirring them uniformly, and then dispersing the above powders with an organic solvent 5-50 times the mass of the solid powder, and vigorously dispersing the above solid-liquid mixture for no less than 3 hours to form a uniform slurry; the organic solvent is selected from one or more of acetone, ethanol, methanol, and N-methylpyrrolidone;
[0017] S6: filtering the mixed raw material obtained in step S5 and washing the filter cake with anhydrous ethanol for 2-3 times, then drying at 50-80° C. and transferring to an inert atmosphere, heating to 450-600° C. and treating at high temperature for 2 hours;
[0018] S7: Grind the catalyst obtained in step S6 into powder to obtain Ni-Fe-La / CNTs-MoC 2 catalyst.
[0019] Preferably, the application steps include: (1) turning on microwave radiation, with a microwave radiation power density of 100-300 kW / m 3 1-10h -1 The ethanol aqueous solution or C1-C3 mixed alcohol aqueous solution containing ethanol is pumped into the catalyst bed at a mass space velocity of 1000 ℃, and the temperature of the catalyst bed is raised to 250-500℃ and maintained for 15-30 minutes under microwave radiation to fully activate the catalyst;
[0020] (2) After the catalyst is activated, -1 The mass space velocity is pumped into the ethanol aqueous solution with a water-to-alcohol molar ratio of 3-6 or the C1-C3 mixed alcohol aqueous solution containing ethanol at 110-200kW / m 3 The microwave radiation power drives the alcohol / water solution to undergo catalytic reforming reaction in the range of 390-470°C.
[0021] Preferably, in the C1-C3 mixed alcohol containing ethanol, the molar proportion of methanol in the mixed alcohol is 0-50%; the molar proportion of propanol and isopropanol in the mixed alcohol is 0-25%.
[0022] Preferably, in step (2), the water-to-alcohol ratio of the ethanol aqueous solution or the C1-C3 mixed alcohol aqueous solution containing ethanol raw material is 4.
[0023] The present invention adopts microwave heating as a typical non-contact direct heating method. Microwaves directly transfer energy to the active sites of the catalytic reaction in the form of electromagnetic waves, which has the advantages of fast heating rate, selective heating and high energy efficiency. The catalyst material mainly converts the microwaves it absorbs into two parts. In addition to the part converted into heat, the other part is stored in the catalyst in the form of electrical potential energy. The energy stored in the form of electrical potential energy will induce the formation of a built-in electric field inside the catalyst, thereby generating a polarization effect. The polarization effect is conducive to promoting the breaking of chemical bonds such as CH bonds and may be conducive to improving hydrogen selectivity.
[0024] In addition, microwaves, as a form of energy that can be efficiently generated from electricity, also provide a solution for the consumption of unstable renewable electricity such as solar power and wind power. That is, by generating microwaves from unstable green electricity and driving the alcohol steam reforming hydrogen production process, zero-carbon production of hydrogen can be achieved. Moreover, bioethanol in C1-C3 low-carbon alcohols has a wide range of sources and is a renewable energy source. It is more sustainable to use it as a raw material for reforming hydrogen. In summary, microwave-driven steam reforming of ethanol or low-carbon mixed alcohols containing ethanol to produce hydrogen has important value and advantages.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. Using microwave radiation to drive the low-carbon alcohol-water reforming reaction greatly reduces the reaction temperature of alcohol-water steam reforming, and the selective heating of microwaves improves energy utilization and reduces energy loss. Unstable renewable electricity such as wind and photovoltaics can be converted into H 2 As chemical energy storage, electricity-hydrogen energy conversion is realized. Under the condition of direct pumping of alcohol-water solution driven by microwaves, efficient in-situ reduction of the catalyst can be achieved in a short time. The reforming hydrogen production reaction has a fast response speed, which is extremely beneficial for the application scenario of instant hydrogen use.
[0027] 2. The catalyst of the present invention can cause ethanol or C1-C3 mixed alcohol aqueous solution containing ethanol to undergo reforming reaction under microwave drive. Under the preferred microwave reaction conditions of 470°C or below, the H 2 The yield reached 4.91 mol, the alcohol conversion rate reached more than 90%, and the CH 4The molar content of CO can be reduced to below 5%, which is not only suitable for pure ethanol / water binary mixture as raw material, but also can effectively process C1-C3 mixed alcohol raw materials containing ethanol, realize the efficient utilization of low-carbon mixed alcohol, avoid the separation and purification of low-carbon mixed alcohol, and thus reduce process costs. It broadens the source of raw materials for reforming hydrogen production, which is very beneficial to improve the economy and sustainability of the hydrogen production process.
[0028] 3. In the reforming catalyst provided by the present invention, the carbon nanotubes with a high degree of graphitization help to improve the conductivity of the catalyst under microwave radiation, which is beneficial to enhancing the reforming hydrogen production performance from the perspective of conductivity. The introduction of molybdenum carbide can further improve the alcohol conversion rate and further effectively reduce the by-product CH 4 and CO selectivity.
[0029] 4. Microwave-driven reforming reaction devices can be miniaturized. The hydrogen-rich gas produced by reforming ethanol or C1-C3 mixed alcohols containing ethanol can be used in small-scale flexible hydrogen use scenarios such as hydrogen fuel cell distributed power stations, in-situ hydrogen production in hydrogen refueling stations, and on-board hydrogen production of hydrogen fuel cell vehicles. It has great application potential and helps solve the problems of difficulty and high cost in hydrogen transportation. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a microwave-driven alcohol steam reforming hydrogen production system and catalyst information diagram; including: 1-raw material tank; 2-liquid pump; 3-microwave reactor; 4-heat exchange system; 5-gas-liquid separation unit; 6-drying unit; 7-flow meter; 8-H 2 Purification unit;
[0031] Figure 2 Characterization of 1# carbon nanotubes: (a) Raman spectrum; (b) thermogravimetric analysis spectrum; (c) resistivity curve; (d) SEM micromorphology;
[0032] Figure 3 Characterization of 2# carbon nanotubes: (a) Raman spectrum; (b) thermogravimetric analysis spectrum; (c) resistivity curve; (d) SEM micromorphology;
[0033] Figure 4 It is MoC 2 Particle size distribution diagram;
[0034] Figure 5 This is the XRD spectrum of the catalyst prepared in Example 4. DETAILED DESCRIPTION
[0035] The present invention will be combined with the specific data of the implementation examples to clearly and completely describe and illustrate the technical solutions of the present invention. Based on the implementation examples in the present invention, all other implementation plans obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0036] The present invention provides an application of a nickel-iron-lanthanum ternary metal supported catalyst in a microwave-driven steam reforming hydrogen production reaction of ethanol or a C1-C3 mixed alcohol containing ethanol. The active component of the nickel-iron-lanthanum ternary metal supported catalyst is Ni-Fe-La, the carrier is a moderately graphitized carbon nanotube, and the auxiliary agent is molybdenum carbide. The steps of preparing the catalyst include:
[0037] S1: According to NiO and Fe 2 O 3 The mass ratio is 0.5-1, La 2 O 3 Precursors of nickel oxide, iron oxide and lanthanum oxide are weighed and mixed respectively, accounting for 3-15% by mass in the active component, deionized water of 2-5 times the mass of the above mixture is added and stirred and dispersed, and then graphitized carbon nanotubes are added in a mass ratio of 0.33-1 to the active component, stirred evenly and ultrasonicated for 2h;
[0038] S2: stirring the mixed raw material obtained in step S1 at room temperature for 3 hours to allow the metal active components to be better dispersed and impregnated on the graphitized carbon nanotubes; after 3 hours, stirring and heating are started to evaporate the water until the material becomes a viscous colloidal slurry, and then transferred to an air environment at 100-160°C for further drying;
[0039] S3: Transfer the catalyst precursor obtained in step S2 into an inert atmosphere, raise the temperature to 400-650° C. and maintain for 2-3 hours;
[0040] S4: grinding the catalyst obtained in step S3 into powder with a particle size of 2-500 μm to obtain a Ni-Fe-La / CNTs supported catalyst;
[0041] S5: mixing the Ni-Fe-La / CNTs supported catalyst obtained in step S4 with molybdenum carbide and pre-stirring them uniformly, and then dispersing the above powders with an organic solvent 5-50 times the mass of the solid powder, and vigorously dispersing the above solid-liquid mixture for no less than 3 hours to form a uniform slurry; the organic solvent is selected from one or more of acetone, ethanol, methanol, and N-methylpyrrolidone;
[0042] S6: filtering the mixed raw material obtained in step S5 and washing the filter cake with anhydrous ethanol for 2-3 times, then drying at 50-80° C. and transferring to an inert atmosphere, heating to 450-600° C. and treating at high temperature for 2 hours;
[0043] S7: Grind the catalyst obtained in step S6 into powder to obtain Ni-Fe-La / CNTs-MoC 2 catalyst.
[0044] use Figure 1 The microwave-driven alcohol steam reforming hydrogen production system shown in the figure performs a hydrogen production reaction by steam reforming ethanol or a C1-C3 mixed alcohol containing ethanol. A set proportion of ethanol or a C1-C3 mixed alcohol aqueous solution containing ethanol is stored in a raw material tank 1, and a liquid pump 2 is used to pump the raw material 1 at a rate of 1-10 hours. -1 The mass space velocity is pumped to the microwave reactor 3 to fully contact with the catalyst of the present invention. 3 The temperature is raised to 450°C under microwave radiation power density and maintained for 10-30 minutes to achieve in-situ activation and achieve the highest activity. After the catalyst is activated, ethanol or C1-C3 mixed alcohol aqueous solution containing ethanol is heated for 2-10 hours. -1 The mass space velocity was pumped into the microwave reactor 3 and the 3 The microwave radiation power density is 390-470℃ and the catalytic reforming hydrogen production reaction occurs. After the reforming reaction gas flows through the heat exchange system 4 for cooling and the gas-liquid separation unit 5 for gas-liquid separation, the liquid phase is pumped back to the raw material tank 1 by the liquid pump 2 and reused as the reforming hydrogen production raw material together with fresh ethanol or C1-C3 mixed alcohol aqueous solution containing ethanol. The gas phase product is roughly dried by the drying unit 6 and then measured and analyzed by the flow meter 7 to obtain the gas product yield and composition, and the alcohol conversion rate is calculated and determined. Then the reforming gas phase product is passed through H 2 Purification unit 8 separates and purifies to obtain high-purity H 2 product.
[0045] The catalytic effect of the catalyst will be explained in detail below in combination with comparative examples and examples.
[0046] Comparative Example 1
[0047] (1) Weigh 10.07 g of copper nitrate trihydrate and 6.09 g of zinc nitrate hexahydrate (the corresponding mass ratio of CuO to ZnO is 2:1) and grind them into a paste in a mortar and place them in a 120°C oven for drying. Finally, heat the temperature to 400°C in a muffle furnace and calcine for 2 h. After the material cools down, take it out and grind it into powder for later use.
[0048] (2) Take 0.67 g of the product of step (1), and then take 0.33 g of 1# carbon nanotube (tube diameter 15-25 nm, tube length 5-15 μm, its microscopic morphology, thermogravimetric analysis spectrum, resistivity curve and Raman spectrum are as follows: Figure 2The two were mechanically ground in a mortar and then loaded into a microwave reactor. Then, an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 was used as the raw material, and the feed rate was maintained at 0.06 mL / min and 150 kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 410-450°C. The results are shown in Table 1.
[0049] Table 1 Comparative Example 1 Reforming Hydrogen Production Results
[0050]
[0051] Comparative Example 2
[0052] (1) Weigh 6.66 g of nickel nitrate hexahydrate, heat it to 400° C. in an air atmosphere in a muffle furnace and calcine it for 2 h. After cooling, take it out and grind it into powder for later use.
[0053] (2) Take 0.67 g of the product of step (1) and 0.33 g of carbon nanotube #1, grind them evenly in a mortar, and then load them all into a microwave reactor. Then, take an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 as the raw material, maintain a feed rate of 0.06 mL / min and a feed speed of 150 kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 410-450°C. The results are shown in Table 2.
[0054] Table 2 Comparative Example 2 Reforming Hydrogen Production Results
[0055]
[0056] Comparative Example 3
[0057] (1) Weigh 5.00 g of nickel acetate tetrahydrate and 7.58 g of ferric nitrate nonahydrate (corresponding NiO:Fe 2 O 3 The mixture was ground into a paste in a mortar and dried in an oven at 120°C, and then transferred to a muffle furnace and heated to 400°C for calcination for 2 hours. After the temperature dropped, the mixture was taken out and ground into powder for later use.
[0058] (2) Take 0.67 g of the product of step (1) and 0.33 g of carbon nanotube #1, grind them evenly in a mortar, and then load them all into a microwave reactor. Then, take an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 as the raw material, maintain a feed rate of 0.06 mL / min and a speed of 150 kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 3.
[0059] Table 3 Comparative Example 3 Reforming Hydrogen Production Results
[0060]
[0061] As shown in Table 1, the catalytic performance of the highly efficient Cu / Zn catalyst commonly used for methanol / steam reforming is extremely weak for ethanol / steam reforming. The conversion rate of ethanol and H 2 The selectivity is about 50%, indicating that the Cu / Zn catalyst system is not suitable for steam reforming of ethanol or C1-C3 low-carbon mixed alcohols containing ethanol. The results of Comparative Example 2 show that when only Ni is used as the catalyst active component, the ethanol conversion rate is only about 50%, and the by-product CH 4 The content is as high as 27%, resulting in low hydrogen selectivity and yield. Therefore, pure Ni is not an ideal catalyst for ethanol steam reforming. Analysis of the results of Comparative Examples 2 and 3 shows that the Ni-Fe catalyst not only improves the ethanol conversion rate, but also significantly reduces CH 4 The selectivity of by-products is to convert CH 4 The molar content of CO was kept below 10%.
[0062] Example 1
[0063] (1) Weigh 5.28 g of nickel acetate tetrahydrate, 15.99 g of ferric nitrate nonahydrate, and 0.67 g of lanthanum nitrate hexahydrate (corresponding to NiO:Fe 2 O 3 Mass ratio 1:2, La 2 O 3 The mixture was evenly ground in a mortar and dried in an oven at 120°C to a paste. The paste was then heated in a muffle furnace N 2 The temperature is raised to 400°C at a rate of 5-10°C / min in the atmosphere and calcined for 2 hours. After the material cools down, it is taken out and ground into powder for later use.
[0064] (2) Take 0.67 g of the product of step (1) and 0.33 g of carbon nanotube #1, grind them evenly in a mortar, and then load them into a microwave reactor. Then, use an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 as the raw material, maintain a feed rate of 0.06 mL / min and a speed of 150 kW / m 3 The microwave radiation power density was used to investigate the hydrogen production performance of ethanol aqueous solution reforming in the temperature range of 390-470°C. The results are shown in Table 4.
[0065] Table 4 Hydrogen production results from reforming of Example 1
[0066]
[0067]
[0068] Comparing Table 3 and Table 4, it can be seen that the introduction of La 2 O 3 It can significantly improve the ethanol conversion rate and convert the by-product CH in the product gas stream into 4 The molar contents of H and CO were maintained at a level comparable to that of pure Ni-Fe catalyst, both at 10 mol%. 2 The yield.
[0069] Example 2
[0070] Take 0.67g of the product of step (1) in Example 1, and then take 0.33g of 2# carbon nanotubes (tube diameter 8-15nm, tube length 10-50μm, its microscopic morphology, thermogravimetric analysis spectrum, resistivity curve and Raman spectrum are as follows: Figure 3 The two were mechanically ground in a mortar and then loaded into a microwave reactor. Then, an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 was used as the raw material, and the feed rate was maintained at 0.06 mL / min and 150 kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 5.
[0071] Table 5 Example 2 reforming hydrogen production results
[0072]
[0073] Comparing Tables 4 and 5, it can be seen that the use of 2# carbon nanotubes significantly reduced the byproduct CH 4 and CO in the reformed product gas stream, which significantly increases the H 2 Product selectivity. Figure 1 and attached Figure 2 The Raman characterization results of carbon nanotubes 1# and 2# in the graphitization degree of carbon nanotubes (measured in I D / I G Ratio measurement; Among them, the I D / I G The ratios are 0.545 and 0.867 respectively) have a significant effect on the reforming hydrogen production performance of the catalyst under microwave field.
[0074] Example 3
[0075] Take 0.67g of the product of step (1) in Example 1, and then take 0.22g of 2# carbon nanotubes, 0.11g of molybdenum carbide (MoC 2 ), and its particle size distribution is as follows Figure 4As shown, Dx(10)=2.60μm, Dx(50)=7.80μm, Dx(90)=53.63μm (generally, the smaller the particle size of molybdenum carbide particles, the higher the activity). Then the three were mechanically ground evenly in a mortar and all loaded into a microwave reactor. Finally, an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 was used as the raw material, and the feed rate was maintained at 0.06mL / min and 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 6.
[0076] Table 6 Example 3 reforming hydrogen production results
[0077]
[0078] Comparing Tables 6 and 5, it can be seen that the introduction of molybdenum carbide has a significant effect on the by-product CH 4 The selectivity of CO and CO was not significantly affected, but the ethanol conversion rate was further significantly improved. For example, the ethanol conversion rate at 430°C was significantly increased from 79.90% to 90.48%.
[0079] Example 4
[0080] (1) Weigh 5.28 g of nickel acetate tetrahydrate, 15.99 g of ferric nitrate nonahydrate, and 0.67 g of lanthanum nitrate hexahydrate (corresponding to NiO:Fe 2 O 3 Mass ratio 1:2, La 2 O 3 5% by mass) in a beaker, add 50mL of deionized water to fully dissolve, then add 1.67g of 2# carbon nanotubes and ultrasonicate for 2h. After stirring the obtained mixed raw materials at room temperature for 3h, turn on the heating to evaporate the water until the material becomes a viscous colloidal slurry, and then transfer it to an air environment of 100-160℃ for further drying; finally, transfer the catalyst precursor to an inert atmosphere and heat it to 400-650℃ at a heating rate of 5-10℃ / min for 2-3h. After cooling, grind the material into powder in a mortar to obtain the 2# carbon nanotube-loaded Ni-Fe-La catalyst (named Ni-Fe-La / CNTs) prepared by the impregnation method.
[0081] The SEM image of Ni-Fe-La / CNTs catalyst is shown in Figure 1 The state and microscopic morphology of the catalyst can be known. The results show that the active components are evenly dispersed on the carbon nanotube carrier, and the carbon nanotubes form a rich microscopic network structure for the entire catalyst, which is beneficial to enhancing the overall conductivity of the catalyst.
[0082] The XRD pattern of Ni-Fe-La / CNTs catalyst is shown in Figure 5It can be seen that compared with the Ni-Fe-La catalyst without carbon nanotube carrier, the XRD diffraction peak of Ni-Fe-La / CNTs is obviously derived, the diffraction peak width becomes larger and the intensity becomes weaker, so that adjacent peaks overlap to form a wider peak. The derived XRD diffraction peak further illustrates the improvement of the dispersion of the active components of the catalyst.
[0083] (2) Take 0.89 g of the product of step (1) and 0.11 g of molybdenum carbide, grind them evenly in a mortar and load them all into a microwave reactor. Finally, take an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 as the raw material, maintain a feed rate of 0.06 mL / min and a speed of 150 kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 7.
[0084] Table 7 Example 4 reforming hydrogen production results
[0085]
[0086] Compared with Example 3, Example 4 changes the matching mode of Ni-Fe-La active components and carbon nanotubes. Figure 5 The XRD results of Ni-Fe-La (without carrier) and Ni-Fe-La / CNTs further confirmed that the catalyst prepared by the impregnation method improved the dispersion of Ni-Fe-La active components, increased the ethanol conversion rate and maintained the byproduct CH 4 and stabilization of CO selectivity.
[0087] Example 5
[0088] Weigh 0.89g of the 2# carbon nanotube-loaded Ni-Fe-La catalyst prepared in step (1) of Example 4, and then take 0.11g of molybdenum carbide, and then disperse the two in 20g of N-methylpyrrolidone solvent, and use ultrasound and stirring to vigorously disperse the above solid-liquid mixture for 3h to form a uniform slurry; filter the obtained mixed raw material and wash the filter cake with anhydrous ethanol 2-3 times and dry it at low temperature (temperature between 50-80℃), transfer it to an inert atmosphere and heat it to 450-600℃ at a heating rate of 5-10℃ / min for high temperature treatment for 2h; after cooling, grind it evenly in a mortar and load it all into a microwave reactor. Finally, use an ethanol aqueous solution with a water-to-alcohol molar ratio of 4:1 as the raw material, maintain a feed rate of 0.06mL / min and a heating rate of 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 8.
[0089] Table 8 Example 5 reforming hydrogen production results
[0090]
[0091]
[0092] Comparison of Examples 4 and 5 shows that changing MoC 2 The mixing mode of MoC and Ni-Fe-La / CNTs has no significant effect on the performance of the catalyst for hydrogen production from ethanol water reforming under microwave. 2 Both mechanical mixing and solvent-assisted dispersion of Ni-Fe-La / CNTs can obtain efficient Ni-Fe-La / CNTs and MoC 2 Composite catalyst system.
[0093] Example 6
[0094] Take 0.67g of the product of step (1) in Example 1, and then take 0.22g of 2# carbon nanotubes and 0.11g of molybdenum carbide respectively, then grind them evenly in a mortar and load them all into a microwave reactor. Finally, a mixed alcohol aqueous solution with a water-to-alcohol molar ratio of 4:1 and a molar mass of ethanol:methanol = 2:1 is used as the raw material, and the feed rate is maintained at 0.06mL / min and 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-450°C. The results are shown in Table 9.
[0095] Table 9 Example 6 Reforming Hydrogen Production Results
[0096]
[0097] Example 7
[0098] Take 0.67g of the product of step (1) in Example 1, and then take 0.22g of 2# carbon nanotubes and 0.11g of molybdenum carbide respectively, then grind them evenly in a mortar and load them all into a microwave reactor. Finally, a mixed alcohol aqueous solution with a water-to-alcohol molar ratio of 4:1 and a molar mass of ethanol:methanol = 1:1 is used as the raw material, and the feed rate is maintained at 0.06mL / min and 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-450°C. The results are shown in Table 10.
[0099] Table 10 Example 7 reforming hydrogen production results
[0100]
[0101]
[0102] Example 8
[0103] Take 0.67g of the product of step (1) in Example 1, and then take 0.22g of 2# carbon nanotubes and 0.11g of molybdenum carbide respectively, then grind the three together in a mortar and load them all into a microwave reactor. Finally, a mixed alcohol aqueous solution with a water-to-alcohol molar ratio of 4:1 and a molar mass of ethanol:isopropanol = 8:1 was used as the raw material, and the feed rate was maintained at 0.06mL / min and 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 430-470°C. The results are shown in Table 11.
[0104] Table 11 Hydrogen production results from reforming of Example 8
[0105]
[0106] Comparing the reforming hydrogen production results of Examples 3, 6 and 8, it can be seen that the catalyst still has obvious reforming activity for C3 alcohols with high reforming difficulty, such as isopropanol, under the radiation of microwaves. 4 The content of by-products has increased to a certain extent, but the content of CO by-product has decreased significantly and the total content of the two can still be maintained below 20%.
[0107] Example 9
[0108] Take 0.67g of the product of step (1) in Example 1, and then take 0.22g of 2# carbon nanotubes and 0.11g of molybdenum carbide respectively, then grind them evenly in a mortar and load them all into a microwave reactor. Finally, a mixed alcohol aqueous solution with a water-to-alcohol molar ratio of 4:1 and a molar mass of methanol: ethanol: isopropanol = 1:8:1 is used as the raw material, and the feed rate is maintained at 0.06mL / min and 150kW / m 3 The microwave radiation power density was used to investigate the reforming hydrogen production performance in the temperature range of 390-470°C. The results are shown in Table 12.
[0109] Table 12 Experimental results of Example 9
[0110]
[0111]
[0112] Comparison of Examples 3, 6, 8 and 9 shows that the mixed low-carbon alcohols of C1-C3 increase the complexity of the reforming reaction, but the catalyst of the present invention still has significant activity and good H for the reforming reaction of the three alcohols. 2 Compared with Example 3, Example 9 shows that the alcohol conversion rate is still as high as 85% at 450°C and CH 4The content of H was maintained at a low level of 5 mol.%, only the molar content of CO by-product increased but also remained below 10 mol.%, 2 The selectivity was not significantly affected.
[0113] In summary, the present invention utilizes the synergistic effect of the thermal effect and the non-thermal effect of microwaves to significantly reduce the steam reforming temperature of ethanol or C1-C3 low-carbon mixed alcohols containing ethanol to 390-470°C. The reduction in reforming temperature also reduces the risk of catalyst sintering and reduces the energy loss of the process to improve energy utilization efficiency. In addition, from the perspective of reaction equilibrium, the reduction in reforming temperature is conducive to the positive movement of the conversion reaction of CO by-products and water vapor, reducing the selectivity of CO by-products. Based on Ni-based catalysts, Fe is introduced to form Ni-Fe alloys with Ni, which improves the dispersion of Ni-based catalysts and can effectively inhibit CO / CO 2 Methanation reaction and sintering of active components. When Ni is in a highly dispersed state or has a strong interaction with the carrier, its reduction temperature will be significantly higher than that of pure NiO. The introduction of Fe can reduce the Ni reduction temperature and promote the reduction of Ni. At the same time, since Fe has a strong affinity for oxygen, the formed Ni-Fe alloy can be oxidized by water vapor in the early stage of the reaction to generate γ-Fe 2 O 3 , which can promote the conversion of ethoxy groups to acetoxy groups, thereby inhibiting the production and subsequent decomposition of acetaldehyde, a precursor of methane, and γ-Fe 2 O 3 It can also react with carbon deposits, significantly improving the anti-coking ability of Ni-based catalysts and improving their stability. 2 O 3 Strong oxygen carrying capacity, in Fe-La 2 O 3 There will also be a small amount of γ-Fe 2 O 3 Generate. And La 2 O 3 The basic sites can modify the Ni-based catalyst to promote its dispersion, prevent Ni metal particles from agglomerating and sintering, and help improve H 2 Yield.
[0114] Absorption and response to microwaves are another important aspect of the steam reforming hydrogen production catalyst. The present invention disperses the above-mentioned Fe and La modified Ni-based catalyst active components with carbon nanotubes having good graphitization degree, high specific surface area, high conductivity and good microwave absorption and response capabilities to form a series of Ni-Fe-La reforming catalysts (Ni-Fe-La / CNTs). The high specific surface area of the carbon nanotubes promotes the high dispersion of the Ni-Fe-La active components and improves the reforming catalytic activity and life of the catalyst. At the same time, the one-dimensional linear structure of the carbon nanotubes is conducive to the formation of a rich high-conductivity network of the catalyst, which is conducive to the electron transfer generated under the polarization of microwave radiation, thereby enhancing the catalytic reforming hydrogen production performance of the catalyst under the microwave field.
[0115] In addition, molybdenum carbide (MoC 2 ) components to further improve the conversion rate of alcohol and the product H in the process of hydrogen production by steam reforming of ethanol and C1-C3 mixed alcohols containing ethanol 2 The above catalyst can be directly activated to a highly active state in situ by microwave radiation under the condition of introducing alcohol / water reforming hydrogen production raw materials, avoiding the need for external H in ordinary thermal processes. 2 This tedious step of pre-reducing the catalyst improves the flexibility and operational elasticity of the steam reforming process for hydrogen production from ethanol or C1-C3 mixed alcohols containing ethanol, and can effectively solve the problem of slow response speed of traditional heating in distributed alcohol / steam reforming hydrogen production application scenarios that require rapid start and stop.
[0116] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. Application of nickel-iron-lanthanum ternary supported catalyst in microwave-driven steam reforming of ethanol or C1-C3 mixed alcohol containing ethanol to produce hydrogen, characterized in that: The active component of the nickel-iron-lanthanum ternary metal supported catalyst is Ni-Fe-La, the carrier is graphitized carbon nanotubes, the carbon content of the carbon nanotubes is ≥99.9%, the tube diameter is 8-15nm, the tube length is 10-50μm, and 0.01≦I D / I G ≦1.0, the auxiliary agent is molybdenum carbide, and the catalyst is composed of the following components in weight percentage: 18-22% nickel oxide, 37-44% iron oxide, 2-11% lanthanum oxide, 22-33% carbon nanotubes, and 11-16.5% molybdenum carbide; the added amount of molybdenum carbide is 0.5-0.75 times the weight of the carbon nanotubes.
2. The use according to claim 1, characterized in that: The particle size of the molybdenum carbide is 0.01-200 μm.
3. The use according to claim 1, characterized in that: The preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include: (1) using water as a solvent, graphitized carbon nanotubes as a carrier, and precursors of nickel oxide, iron oxide, and lanthanum oxide as raw materials for impregnation synthesis to obtain a Ni-Fe-La / CNTs supported catalyst; (2) based on the Ni-Fe-La / CNTs supported catalyst, introducing a molybdenum carbide component, and using a dry ball milling mechanical mixing method or an organic solvent-assisted dispersion method to evenly mix the molybdenum carbide and the Ni-Fe-La / CNTs catalyst to obtain a Ni-Fe-La / CNTs-MoC2 catalyst.
4. The use according to claim 1, characterized in that: The preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include: (1) firstly using nickel oxide, iron oxide and lanthanum oxide precursors as raw materials, grinding and calcining to obtain catalyst active components, and then mechanically grinding them with carrier graphitized carbon nanotubes to obtain Ni-Fe-La / CNTs supported catalyst; (2) based on the Ni-Fe-La / CNTs supported catalyst, introducing molybdenum carbide component, using dry ball milling mechanical mixing method or organic solvent assisted dispersion method to mix molybdenum carbide and Ni-Fe-La / CNTs catalyst evenly, to obtain Ni-Fe-La / CNTs-MoC2 catalyst.
5. The use according to claim 3 or 4, characterized in that: The precursors of the nickel oxide, iron oxide and lanthanum oxide are one or more of the nitrates and hydrates thereof, acetates and hydrates thereof or hydroxides of the corresponding metals.
6. The use according to claim 5, characterized in that: The precursors of the nickel oxide, iron oxide and lanthanum oxide are nickel acetate hydrate, iron nitrate hydrate and lanthanum nitrate hydrate respectively.
7. The use according to claim 1 or 3, characterized in that: The preparation steps of the nickel-iron-lanthanum ternary metal supported catalyst include: S1: According to the mass ratio of NiO to Fe2O3 of 0.5-1, La2O3 accounts for 3-15% of the mass in the active component, respectively weigh the precursors of nickel oxide, iron oxide, and lanthanum oxide, mix them, add 2-5 times the mass of the above mixture of deionized water, stir and disperse, then add graphitized carbon nanotubes, stir evenly and ultrasonicate for 2h; the mass ratio of graphitized carbon nanotubes to active components is 0.33-1; S2: stirring the mixed raw material obtained in step S1 at room temperature for 3 hours to allow the metal active components to be better dispersed and impregnated on the graphitized carbon nanotubes; after 3 hours, stirring and heating are started to evaporate the water until the material becomes a viscous colloidal slurry, and then transferred to an air environment at 100-160°C for further drying; S3: Transfer the catalyst precursor obtained in step S2 into an inert atmosphere, raise the temperature to 400-650° C. and maintain for 2-3 hours; S4: grinding the catalyst obtained in step S3 into powder with a particle size of 2-500 μm to obtain a Ni-Fe-La / CNTs supported catalyst; S5: mixing the Ni-Fe-La / CNTs supported catalyst obtained in step S4 with molybdenum carbide and pre-stirring them uniformly, and then dispersing the above powders with an organic solvent 5-50 times the mass of the solid powder, and vigorously dispersing the above solid-liquid mixture for no less than 3 hours to form a uniform slurry; the organic solvent is selected from one or more of acetone, ethanol, methanol, and N-methylpyrrolidone; S6: filtering the mixed raw material obtained in step S5 and washing the filter cake with anhydrous ethanol for 2-3 times, then drying at 50-80° C. and transferring to an inert atmosphere, heating to 450-600° C. and treating at high temperature for 2 hours; S7: Grind the catalyst obtained in step S6 into powder to obtain a Ni-Fe-La / CNTs-MoC2 catalyst.
8. The use according to claim 1, characterized in that: The steps of the application include: (1) Turn on microwave radiation, with a microwave radiation power density of 100-300kW / m 3 1-10h -1 The ethanol aqueous solution or C1-C3 mixed alcohol aqueous solution containing ethanol is pumped into the catalyst bed at a mass space velocity of 1000 ℃, and the temperature of the catalyst bed is raised to 250-500℃ and maintained for 15-30 minutes under microwave radiation to fully activate the catalyst; (2) After the catalyst is activated, -1 The mass space velocity is pumped into the ethanol aqueous solution with a water-to-alcohol molar ratio of 3-6 or the C1-C3 mixed alcohol aqueous solution containing ethanol at 110-200kW / m 3 The microwave radiation power drives the alcohol / water solution to undergo catalytic reforming reaction in the range of 390-470°C.
9. The use according to claim 8, characterized in that: In the C1-C3 mixed alcohol containing ethanol, the molar proportion of methanol in the mixed alcohol is 0-50%; the molar proportion of propanol and isopropanol in the mixed alcohol is 0-25%.
10. The use according to claim 8, characterized in that: In step (2), the water-to-alcohol molar ratio of the ethanol aqueous solution or C1-C3 mixed alcohol aqueous solution containing ethanol is 4.