A high strength, toughness and hardness (TiZrVNb)C x Preparation method of multi-phase multi-component carbide ceramic material

High-strength, tough and hard (TiZrVNb) Cx complex-phase multi-component carbide ceramic materials are prepared through high-energy ball milling and sintering technology, which solves the bottleneck of improving the mechanical properties of single-phase multi-component carbide ceramics and achieves high density and excellent mechanical properties. Meet the demand for high-performance ceramic materials in the aerospace and nuclear energy sectors.

CN118084495BActive Publication Date: 2024-10-29HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410151110.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-10-29
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

The mechanical properties of existing single-phase multi-component carbide ceramics are difficult to further improve and cannot meet the stringent requirements for high-performance ceramic materials in the aerospace and nuclear energy fields.

Method used

High-energy ball milling and sintering technology are used to prepare high-strength, tough and hard (TiZrVNb) Cx multi-phase multi-component carbide ceramic materials through in-situ solid-state reaction and spontaneous phase decomposition, and control its microstructure and stoichiometric ratio to achieve grain refinement. and mechanical properties improvement.

Benefits of technology

The prepared (TiZrVNb)Cx complex-phase multi-component carbide ceramic material has high density, excellent strength and hardness, can meet the needs of nuclear reactors and ultra-high temperature fields, and significantly improves the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118084495B_ABST
    Figure CN118084495B_ABST
Patent Text Reader

Abstract

A high strength, toughness and hardness (TiZrVNb)C x The invention discloses a method for preparing a multi-phase multi-component carbide ceramic material, which belongs to the technical field of ceramic materials. The purpose of the invention is to solve the technical problem that the mechanical properties of existing single-phase multi-component carbide ceramics are difficult to further improve. The method includes: 1. weighing the required powder; 2. mixing; 3. sintering; 4. demoulding. The high-strength, toughness and hardness (TiZrVNb)C prepared by the invention x The multi-phase multi-component carbide ceramic material is a multi-phase face-centered cubic structure ceramic with phase decomposition characteristics and fine grain size. x The density of multi-phase multi-component carbide ceramic materials is higher than 98.7%, the hardness at room temperature is 35-40GPa, the three-point bending strength is 600-800MPa, and the fracture toughness is 3.2-5.4MPa·m 1 / 2 . It can meet the working requirements in nuclear reactors and ultra-high temperature fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of ceramic materials, and specifically relates to a high-strength, tough and hard (TiZrVNb) C x The invention discloses a method for preparing a multi-phase multi-component carbide ceramic material. Background Art

[0002] With the continuous development of aerospace and nuclear energy, the performance requirements for ultra-high temperature materials have become more and more stringent. Ultra-high temperature ceramics, especially transition metal carbide ceramics, are widely used in aerospace, machinery and metallurgy due to their high melting point, high hardness, low density, good oxidation resistance and high temperature mechanical properties. In recent years, multi-component carbide ceramics have attracted widespread attention due to their special properties brought by their complex composition. Compared with single-component carbide ceramics, the comprehensive performance of multi-component carbide ceramics has been improved.

[0003] However, the research on multi-component carbide ceramics is concentrated on single-phase carbide ceramics, and the research on the mechanical properties of single-phase carbide ceramics has entered a bottleneck stage and is difficult to improve further. Complex-phase multi-component carbide ceramics will have the advantages of both the solid solution hardening of multi-component carbide ceramics and the hardening of complex-phase materials, but the current research on complex-phase multi-component carbide ceramics is very limited. Therefore, it is very important to invent a new type of high-performance complex-phase multi-component carbide ceramic and its preparation method, which can achieve grain refinement, microstructure regulation and comprehensive mechanical property improvement through in-situ solid-phase reaction and spontaneous phase decomposition, so as to meet the increasingly stringent requirements of the aerospace and nuclear energy industries for the performance of new advanced ceramic materials. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problem that the mechanical properties of existing single-phase multi-component carbide ceramics are difficult to further improve, and to provide a high-strength, tough and hard (TiZrVNb)C x The invention discloses a method for preparing a multi-phase multi-component carbide ceramic material.

[0005] The present invention provides a new type of high-performance complex phase multi-component carbide ceramic to meet the performance requirements of aerospace and nuclear energy industries for new advanced ceramic materials.

[0006] A high strength, toughness and hardness (TiZrVNb)C x The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0007] 1. Weigh the required powder:

[0008] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders. Among them, the molar amounts of titanium hydride and zirconium hydride powders are equal, the molar amounts of titanium carbide and zirconium carbide powders are equal, and the molar amounts of niobium carbide and vanadium carbide powders are equal to obtain a mixed powder;

[0009] In step one, the molar ratio of titanium hydride, titanium carbide and niobium carbide is 2(1 - x):(2x - 1):1, where 0.5 < x < 1.0;

[0010] II. Mixing:

[0011] Perform high-energy ball milling on the mixed powder weighed in step one to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and make the powder evenly mixed to obtain the ball-milled mixed powder;

[0012] III. Sintering:

[0013] Place the ball-milled mixed powder in a mold for sintering to obtain a ceramic sintered body;

[0014] IV. Demolding:

[0015] Take out the ceramic sintered body from the mold to obtain high-strength, tough and hard (TiZrVNb)C x composite multi-component carbide ceramic material.

[0016] The (TiZrVNb)C x where the value range of x is 0.5 < x < 1.0, and the molar contents of Ti, Zr, V and Nb are equal.

[0017] The present invention has the following beneficial effects:

[0018] I. The present invention selects hydride powders and carbide powders as the initial powders, mixes them evenly and then sinters them, which can effectively solve the problems of oxygen pollution and oxidation and cold welding that are prone to occur in metal powders during high-energy ball milling, and can realize the adjustable and controllable carbon content to prepare (TiZrVNb)C x composite multi-component carbide ceramics; the existence of carbon vacancies can effectively promote the mass transfer process during sintering, reduce the sintering temperature of the ceramic material, regulate the phase composition and microstructure, effectively refine the grains, and improve the material density. The (TiZrVNb)C x composite multi-component carbide ceramics prepared by the present invention have a density higher than 98.7%, and the significant phase decomposition characteristics endow the material with excellent strength and hardness;

[0019] II. The high-strength, tough and hard (TiZrVNb)C x composite multi-component carbide ceramic material prepared by the present invention is a composite face-centered cubic structure ceramic with phase decomposition characteristics and fine grain size;

[0020] 3. High-strength, tough and hard (TiZrVNb)C prepared by the present invention x Multi-phase multi-component carbide ceramics have the advantages of multi-component carbide ceramics solid solution hardening and multi-phase material hardening. At the same time, the significant phase decomposition makes (TiZrVNb)C x Multi-phase multi-component carbide ceramics have a finer grain size, and the synergistic effect of multiple hardening mechanisms makes the high-strength, toughness and hardness (TiZrVNb)C x The hardness and strength of multi-phase multi-component carbide ceramics have been significantly improved, with a hardness of 35-40 GPa at room temperature, a three-point bending strength of 600-800 MPa, and a fracture toughness of 3.2-5.4 MPa·m 1 / 2 . It can meet the working requirements in nuclear reactors and ultra-high temperature fields.

[0021] The present invention can obtain a high-strength, tough and hard (TiZrVNb) C x Complex phase multi-component carbide ceramic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 3 0.9 XRD patterns of complex phase multi-component carbide ceramic materials;

[0023] Figure 2 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 3 0.9 SEM image of multi-phase multi-component carbide ceramic material;

[0024] Figure 3 for Figure 2 Ti element distribution diagram in;

[0025] Figure 4 for Figure 2 Zr element distribution diagram in;

[0026] Figure 5 for Figure 2 Distribution diagram of V element in;

[0027] Figure 6 for Figure 2 Nb element distribution diagram in.

[0028] Figure 7 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 5 0.8 XRD patterns of complex phase multi-component carbide ceramic materials;

[0029] Figure 8 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 5 0.8SEM image of complex phase multi-component carbide ceramic material. DETAILED DESCRIPTION

[0030] The following examples are intended to further illustrate the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0031] Specific implementation method 1: This implementation method is a high-strength, tough and hard (TiZrVNb) C x The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0032] 1. Weigh the required powder:

[0033] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0034] The molar ratio of titanium hydride, titanium carbide and niobium carbide in step 1 is 2(1-x):(2x-1):1, wherein 0.5<x<1.0;

[0035] 2. Mixing:

[0036] The mixed powder weighed in step 1 is subjected to high-energy ball milling to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a mixed powder after ball milling;

[0037] 3. Sintering:

[0038] The ball-milled mixed powder is placed in a mold for sintering to obtain a ceramic sintered body;

[0039] 4. Demolding:

[0040] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C x Complex phase multi-component carbide ceramic materials.

[0041] Specific embodiment 2: The difference between this embodiment and specific embodiment 1 is that the chemical formulas of the titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders described in step 1 are TiC, ZrC, NbC, VC, TiH 2 and ZrH 2 , the purity is >99.0wt.%. The other steps are the same as those in the first embodiment.

[0042] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the ball-to-material ratio of the high-energy ball mill in step 2 is (10-100):1, the rotation speed of the high-energy ball mill is 300r / min-700r / min, the time of the high-energy ball mill is 10h-40h, and the material of the ball mill jar and the grinding ball is cemented carbide. The other steps are the same as those of specific embodiment 1 or 2.

[0043] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the sintering method described in step 3 is spark plasma sintering. The other steps are the same as those of specific embodiments 1 to 3.

[0044] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the spark plasma sintering process described in step 3 is: heating from room temperature to 2000°C to 2400°C, keeping at 2000°C to 2400°C for 5min to 30min, then cooling to room temperature, the heating rate is 50°C / min to 200°C / min, the cooling rate is 50°C / min to 400°C / min, and the pressure is maintained at 20MPa to 80MPa during the sintering process. The other steps are the same as those of specific embodiments 1 to 4.

[0045] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the sintering method described in step 3 is hot pressing sintering. The other steps are the same as those of specific embodiments 1 to 5.

[0046] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the hot pressing sintering process described in step 3 is: heating from room temperature to 1800°C to 2300°C, keeping at 1800°C to 2300°C for 5min to 120min, then cooling to room temperature, heating rate of 5°C / min to 30°C / min, cooling rate of 5°C / min to 50°C / min, and keeping pressure of 20MPa to 100MPa during sintering. Other steps are the same as those of specific embodiments 1 to 6.

[0047] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: during the sintering process in step 3, an inert gas needs to be continuously introduced to form a protective atmosphere, or a vacuum state needs to be maintained. The other steps are the same as those of specific embodiments 1 to 7.

[0048] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the inert gas is argon, helium or krypton, and the vacuum state is <15 Pa. The other steps are the same as those of specific embodiments 1 to 8.

[0049] Specific Embodiment Ten: The difference between this embodiment and any one of Specific Embodiments One to Nine is that in (TiZrVNb)C x the value range of x is 0.5 < x < 1.0, and the molar contents of Ti, Zr, V, and Nb are equal. Other steps are the same as those in Specific Embodiments One to Nine.

[0050] The following examples are used to verify the beneficial effects of the present invention:

[0051] Example 1: A preparation method of a high-strength, tough and hard (TiZrVNb)C 0.85 composite multi-component carbide ceramic material, which is specifically completed according to the following steps:

[0052] I. Weigh the required powders:

[0053] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders. Among them, the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal to obtain a mixed powder;

[0054] In Step I, the molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders is 3:3:7:7:10:10;

[0055] The purities of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide described in Step I are all > 99.0 wt.%;

[0056] II. Mixing:

[0057] In a vacuum environment, the mixed powder weighed in Step I is subjected to high-energy ball milling to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and make the powder evenly mixed to obtain the ball-milled mixed powder;

[0058] In Step II, the ball-to-powder ratio of the high-energy ball milling is 20:1, the rotation speed of the high-energy ball milling is 600 r / min, the time of the high-energy ball milling is 10 h, and the materials of the ball mill and the grinding balls are both cemented carbide;

[0059] III. Sintering:

[0060] Place the ball-milled mixed powder in a mold and perform spark plasma sintering under argon protection to obtain a ceramic sintered body;

[0061] The process of the spark plasma sintering described in Step III is: heating from room temperature to 2200 °C, holding at 2200 °C for 5 min, then cooling to room temperature, the heating rate is 50 °C / min, the cooling rate is 100 °C / min, and the pressure is maintained at 25 MPa during the sintering process;

[0062] 4. Demolding:

[0063] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.85 Complex phase multi-component carbide ceramic materials.

[0064] Example 1 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.85 The density of the multi-phase multi-component carbide ceramic material is 99.1%, the hardness can reach 39.6GPa, the three-point bending strength is 690MPa, and the fracture toughness is 3.31MPa·m 1 / 2 .

[0065] Example 2: A high strength, toughness and hardness (TiZrVNb)C 0.85 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0066] 1. Weigh the required powder:

[0067] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0068] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders in step 1 is 3:3:7:7:10:10;

[0069] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0070] 2. Mixing:

[0071] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0072] The ball-to-material ratio of the high-energy ball mill described in step 2 is 10:1, the speed of the high-energy ball mill is 700 r / min, the time of the high-energy ball mill is 20 h, and the materials of the ball mill and the grinding balls are both cemented carbide;

[0073] 3. Sintering:

[0074] The ball-milled mixed powder is placed in a mold and hot-pressed and sintered under vacuum conditions to obtain a ceramic sintered body;

[0075] The hot pressing sintering process described in step 3 is: heating from room temperature to 2100°C, keeping at 2100°C for 50 minutes, and then cooling to room temperature, with a heating rate of 20°C / min and a cooling rate of 45°C / min, and maintaining a pressure of 30MPa during the sintering process;

[0076] 4. Demolding:

[0077] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.85 Complex phase multi-component carbide ceramic materials.

[0078] Example 2 High-strength, tough and hard (TiZrVNb)C 0.85 The density of the multi-phase multi-component carbide ceramic material is 99.0%, the hardness can reach 38.9GPa, the three-point bending strength is 678MPa, and the fracture toughness is 3.46MPa·m 1 / 2 .

[0079] Example 3: A high strength, toughness and hardness (TiZrVNb)C 0.9 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0080] 1. Weigh the required powder:

[0081] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0082] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 1:1:4:4:5:5;

[0083] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0084] 2. Mixing:

[0085] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0086] The ball-to-material ratio of the high-energy ball mill described in step 2 is 40:1, the speed of the high-energy ball mill is 400r / min, the time of the high-energy ball mill is 20h, and the materials of the ball mill jar and the grinding balls are both cemented carbide;

[0087] 3. Sintering:

[0088] The ball-milled mixed powder is placed in a mold and spark plasma sintered under argon protection to obtain a ceramic sintered body;

[0089] The spark plasma sintering process described in step 3 is: heating from room temperature to 2300°C, keeping at 2300°C for 15 minutes, and then cooling to room temperature, with a heating rate of 100°C / min and a cooling rate of 150°C / min, and maintaining a pressure of 55MPa during the sintering process;

[0090] 4. Demolding:

[0091] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.9 Complex phase multi-component carbide ceramic materials.

[0092] Example 3 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.9 The density of the multi-phase multi-component carbide ceramic material is 99.4%, the hardness can reach 39.8GPa, the three-point bending strength is 758MPa, and the fracture toughness is 5.31MPa·m 1 / 2 .

[0093] Figure 1 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 3 0.9 XRD patterns of complex phase multi-component carbide ceramic materials;

[0094] from Figure 1 It can be seen that the high-strength, tough and hard (TiZrVNb)C prepared in Example 3 0.9 Three groups of diffraction peaks of carbide solid solution appear in the complex phase multi-component carbide ceramic material, all of which are face-centered cubic structures without any impurity phase, proving that the (TiZrVNb)C 0.9 Complex phase multi-component carbide ceramic materials.

[0095] Figure 2 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 3 0.9 SEM image of multi-phase multi-component carbide ceramic material;

[0096] from Figure 2 It can be seen that the high-strength, tough and hard (TiZrVNb)C prepared in Example 3 0.9 The complex phase multi-component carbide ceramic material has high density and contains three phases with different contrasts. The grain size of the dark phase and the light phase is smaller than that of the gray phase. The dark phase and the light phase present an alternating layered structure and are formed by in-situ decomposition of the gray phase. The grain size distribution of each phase is relatively uniform, and there is no abnormal growth phenomenon.

[0097] Figure 3 for Figure 2Ti element distribution diagram in;

[0098] Figure 4 for Figure 2 Zr element distribution diagram in;

[0099] Figure 5 for Figure 2 Distribution diagram of V element in;

[0100] Figure 6 for Figure 2 Nb element distribution diagram in;

[0101] Figure 3 to Figure 6 It shows that the high strength, toughness and hardness (TiZrVNb) C prepared in Example 3 0.9 In the complex-phase multi-component carbide ceramic material, the metal elements Ti, Zr, V and Nb are evenly distributed in the gray phase without obvious element segregation; in the dark phase, the Ti and V elements are enriched; and in the light phase, the Zr element is enriched; this shows that the contrast difference comes from the difference in the content of metal elements in each phase, which once again proves that complex-phase multi-component carbide ceramic materials can be obtained by adopting this technical solution.

[0102] Example 4: A high strength, toughness and hardness (TiZrVNb)C 0.9 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0103] 1. Weigh the required powder:

[0104] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0105] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 1:1:4:4:5:5;

[0106] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0107] 2. Mixing:

[0108] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0109] The ball-to-material ratio of the high-energy ball mill described in step 2 is 40:1, the speed of the high-energy ball mill is 650 r / min, the time of the high-energy ball mill is 30 h, and the material of the ball mill and the grinding ball are both cemented carbide;

[0110] 3. Sintering:

[0111] The ball-milled mixed powder is placed in a mold and hot-pressed and sintered under argon protection to obtain a ceramic sintered body;

[0112] The hot pressing sintering process described in step 3 is: heating from room temperature to 2300°C, keeping at 2300°C for 120 minutes, then cooling to room temperature, with a heating rate of 20°C / min, a cooling rate of 20°C / min, and a pressure of 75MPa during the sintering process;

[0113] 4. Demolding:

[0114] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.9 Complex phase multi-component carbide ceramic materials.

[0115] Example 4 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.9 The density of the multi-phase multi-component carbide ceramic material is 99.7%, the hardness can reach 39.3GPa, the three-point bending strength is 771MPa, and the fracture toughness is 5.23MPa·m 1 / 2 .

[0116] Example 5: A high strength, toughness and hardness (TiZrVNb)C 0.8 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0117] 1. Weigh the required powder:

[0118] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0119] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 2:2:3:3:5:5;

[0120] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0121] 2. Mixing:

[0122] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0123] The ball-to-material ratio of the high-energy ball mill described in step 2 is 80:1, the speed of the high-energy ball mill is 700 r / min, the time of the high-energy ball mill is 30 h, and the material of the ball mill and the grinding ball are both cemented carbide;

[0124] 3. Sintering:

[0125] The ball-milled mixed powder is placed in a mold and spark plasma sintered under argon protection to obtain a ceramic sintered body;

[0126] The spark plasma sintering process described in step 3 is: heating from room temperature to 2400°C, keeping at 2400°C for 25 minutes, and then cooling to room temperature, with a heating rate of 200°C / min, a cooling rate of 350°C / min, and a pressure of 75MPa during the sintering process;

[0127] 4. Demolding:

[0128] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.8 Complex phase multi-component carbide ceramic materials.

[0129] Figure 7 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 5 0.8 XRD patterns of complex phase multi-component carbide ceramic materials;

[0130] from Figure 7 It can be seen that the high-strength, tough and hard (TiZrVNb)C prepared in Example 5 0.8 Three groups of diffraction peaks of carbide solid solution appear in the complex phase multi-component carbide ceramic material, all of which are face-centered cubic structures without any impurity phase, proving that the (TiZrVNb)C 0.8 Complex phase multi-component carbide ceramic materials.

[0131] Figure 8 The high strength, toughness and hardness (TiZrVNb)C prepared in Example 5 0.8 SEM image of multi-phase multi-component carbide ceramic material;

[0132] from Figure 8 It can be seen that the high-strength, tough and hard (TiZrVNb)C prepared in Example 5 0.8 Complex phase multi-component carbide ceramic materials have high density and exist three phases with different contrasts. The dark phase and the light phase present an alternating layered structure and are formed by in-situ phase decomposition.

[0133] Example 5 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.8The density of the multi-phase multi-component carbide ceramic material is 98.7%, the hardness can reach 37.2GPa, the three-point bending strength is 692MPa, and the fracture toughness is 4.86MPa·m 1 / 2 .

[0134] Example 6: A high strength, toughness and hardness (TiZrVNb)C 0.7 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0135] 1. Weigh the required powder:

[0136] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0137] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 3:3:2:2:5:5;

[0138] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0139] 2. Mixing:

[0140] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0141] The ball-to-material ratio of the high-energy ball mill described in step 2 is 50:1, the speed of the high-energy ball mill is 500r / min, the time of the high-energy ball mill is 40h, and the material of the ball mill and the grinding ball are both cemented carbide;

[0142] 3. Sintering:

[0143] The ball-milled mixed powder is placed in a mold and spark plasma sintered under argon protection to obtain a ceramic sintered body;

[0144] The spark plasma sintering process described in step 3 is: heating from room temperature to 2000°C, keeping at 2000°C for 30 minutes, and then cooling to room temperature, with a heating rate of 100°C / min, a cooling rate of 200°C / min, and a pressure of 45MPa during the sintering process;

[0145] 4. Demolding:

[0146] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.7Complex phase multi-component carbide ceramic materials.

[0147] Example 6 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.7 The density of the multi-phase multi-component carbide ceramic material is 99.4%, the hardness can reach 36.7GPa, the three-point bending strength is 652MPa, and the fracture toughness is 4.52MPa·m 1 / 2 .

[0148] Example 7: A high strength, toughness and hardness (TiZrVNb)C 0.6 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0149] 1. Weigh the required powder:

[0150] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0151] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 4:4:1:1:5:5;

[0152] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0153] 2. Mixing:

[0154] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0155] The ball-to-material ratio of the high-energy ball mill described in step 2 is 40:1, the speed of the high-energy ball mill is 400r / min, the time of the high-energy ball mill is 25h, and the materials of the ball mill and the grinding balls are both cemented carbide;

[0156] 3. Sintering:

[0157] The ball-milled mixed powder is placed in a mold and spark plasma sintered under vacuum conditions to obtain a ceramic sintered body;

[0158] The spark plasma sintering process described in step 3 is: heating from room temperature to 2000°C, keeping at 2000°C for 10 minutes, and then cooling to room temperature, with a heating rate of 40°C / min and a cooling rate of 100°C / min, and maintaining a pressure of 35MPa during the sintering process;

[0159] 4. Demolding:

[0160] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.6 Complex phase multi-component carbide ceramic materials.

[0161] Example 7 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.6 The density of the multi-phase multi-component carbide ceramic material is 99.2%, the hardness can reach 36.4GPa, the three-point bending strength is 647MPa, and the fracture toughness is 4.39MPa·m 1 / 2 .

[0162] Example 8: A high strength, toughness and hardness (TiZrVNb)C 0.55 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0163] 1. Weigh the required powder:

[0164] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0165] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 9:9:1:1:10:10;

[0166] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0167] 2. Mixing:

[0168] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0169] The ball-to-material ratio of the high-energy ball mill described in step 2 is 40:1, the speed of the high-energy ball mill is 400r / min, the time of the high-energy ball mill is 25h, and the materials of the ball mill and the grinding balls are both cemented carbide;

[0170] 3. Sintering:

[0171] The ball-milled mixed powder is placed in a mold and vacuum sintered under vacuum conditions to obtain a ceramic sintered body;

[0172] The vacuum sintering process described in step 3 is: heating from room temperature to 2000°C, keeping at 2000°C for 20 minutes, and then cooling to room temperature, with a heating rate of 15°C / min, a cooling rate of 30°C / min, and a pressure of 75MPa during the sintering process;

[0173] 4. Demolding:

[0174] The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C 0.55 Complex phase multi-component carbide ceramic materials.

[0175] Example 8 Preparation of high strength, toughness and hardness (TiZrVNb)C 0.55 The density of the multi-phase multi-component carbide ceramic material is 99.5%, the hardness can reach 35.4GPa, the three-point bending strength is 622MPa, and the fracture toughness is 3.74MPa·m 1 / 2 .

[0176] Comparative Example 1: A (TiZrHfTa)C 0.8 Multi-component carbide solid solution ceramics are made in the following steps:

[0177] 1. Weigh the required powder:

[0178] Weigh titanium carbide, zirconium carbide, hafnium carbide, tantalum carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of hafnium carbide and tantalum carbide powders are equal, to obtain a mixed powder;

[0179] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, hafnium carbide and tantalum carbide powders described in step 1 is 2:2:3:3:5:5;

[0180] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, hafnium carbide and tantalum carbide in step 1 is > 99.0wt.%;

[0181] 2. Mixing:

[0182] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0183] The ball-to-material ratio of the high-energy ball mill described in step 2 is 40:1, the speed of the high-energy ball mill is 400r / min, the time of the high-energy ball mill is 25h, and the materials of the ball mill and the grinding balls are both cemented carbide;

[0184] 3. Sintering:

[0185] The ball-milled mixed powder is placed in a mold and hot-pressed and sintered under vacuum conditions to obtain a ceramic sintered body;

[0186] The vacuum sintering process described in step 3 is: heating from room temperature to 2000°C, keeping at 2000°C for 20 minutes, and then cooling to room temperature, with a heating rate of 15°C / min, a cooling rate of 30°C / min, and a pressure of 75MPa during the sintering process;

[0187] 4. Demolding:

[0188] The ceramic sintered body is removed from the mold to obtain a (TiZrHfTa)C 0.8 Multi-component carbide solid solution ceramic materials.

[0189] A (TiZrHfTa)C prepared in Comparative Example 1 0.8 The multi-component carbide solid solution ceramic material was characterized, and no phase decomposition structure was observed. It was a single-phase carbide ceramic material with a density of 98.4%, a hardness of 30.1 GPa, a three-point bending strength of 379 MPa, and a fracture toughness of 3.41 MPa·m. 1 / 2 By comparison, it can be found that the (TiZrVNb)C prepared by the technical solution of the present invention has a significant phase decomposition structure. x The density and mechanical properties of complex phase multi-component carbide ceramic materials have significant advantages.

[0190] Comparative Example 2: A (TiZrVNb)C 1.0 The preparation method of the multi-phase multi-component carbide ceramic material is specifically completed according to the following steps:

[0191] 1. Weigh the required powder:

[0192] Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder;

[0193] The molar ratio of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide powders described in step 1 is 0:0:1:1:1:1;

[0194] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and vanadium carbide in step 1 is all > 99.0wt.%;

[0195] 2. Mixing:

[0196] The mixed powder weighed in step 1 is subjected to high-energy ball milling in a vacuum environment to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a ball-milled mixed powder;

[0197] The ball-to-material ratio of the high-energy ball mill described in step 2 is 20:1, the speed of the high-energy ball mill is 600 r / min, the time of the high-energy ball mill is 10 h, and the material of the ball mill and the grinding ball are both cemented carbide;

[0198] 3. Sintering:

[0199] The ball-milled mixed powder is placed in a mold and spark plasma sintered under argon protection to obtain a ceramic sintered body;

[0200] The spark plasma sintering process described in step 3 is: heating from room temperature to 2200°C, keeping at 2200°C for 5 minutes, and then cooling to room temperature, with a heating rate of 50°C / min and a cooling rate of 100°C / min, and maintaining a pressure of 25MPa during the sintering process;

[0201] 4. Demolding:

[0202] The ceramic sintered body is removed from the mold to obtain a (TiZrVNb)C 1.0 Complex phase multi-component carbide ceramic materials.

[0203] A (TiZrVNb)C prepared in Comparative Example 2 1.0 The composite multi-component carbide ceramic material was characterized and no phase decomposition structure was observed. Its density is 98.9%, hardness is 33.1GPa, three-point bending strength is 393MPa, and fracture toughness is 3.66MPa·m 1 / 2 By comparison, it can be found that the (TiZrVNb)C prepared by the technical solution of the present invention has a significant phase decomposition structure. x The mechanical properties of complex phase multi-component carbide ceramic materials have significant advantages.

Claims

1. A high strength, toughness and hardness (TiZrVNb)C x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The preparation method is specifically completed according to the following steps:

1. Weigh the required powder: Weigh titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, the molar numbers of titanium carbide and zirconium carbide powders are equal, and the molar numbers of niobium carbide and vanadium carbide powders are equal, to obtain a mixed powder; The molar ratio of titanium hydride, titanium carbide and niobium carbide in step 1 is 2(1-x):(2x-1):1, wherein 0.5<x<1.0; 2. Mixing: The mixed powder weighed in step 1 is subjected to high-energy ball milling to mix and crush the powder, reduce the particle size of the powder to improve its reaction activity and sintering activity, and mix the powder evenly to obtain a mixed powder after ball milling; 3. Sintering: The ball-milled mixed powder is placed in a mold for sintering to obtain a ceramic sintered body; 4. Demolding: The ceramic sintered body is removed from the mold to obtain a high-strength, tough and hard (TiZrVNb)C x Complex phase multi-component carbide ceramic materials; (TiZrVNb)C as described x In which, the value range of x is 0.5 < x < 1.0, and the molar contents of Ti, Zr, V and Nb are equal.

2. A high strength, toughness and hardness (TiZrVNb) C according to claim 1. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The purity of the titanium carbide, zirconium carbide, niobium carbide, vanadium carbide, titanium hydride and zirconium hydride powders described in step 1 is all >99.0wt.%.

3. A high strength, toughness and hardness (TiZrVNb) C according to claim 1. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The ball-to-material ratio of the high-energy ball mill described in step 2 is (10-100):1, the rotation speed of the high-energy ball mill is 300r / min-700r / min, the time of the high-energy ball mill is 10h-40h, and the material of the ball mill jar and the grinding balls are both cemented carbide.

4. A high strength, toughness and hardness (TiZrVNb) C according to claim 1. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The sintering method described in step three is spark plasma sintering.

5. A high strength, toughness and hardness (TiZrVNb) C according to claim 4 x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The spark plasma sintering process described in step three is: heating from room temperature to 2000°C~2400°C, keeping at 2000°C~2400°C for 5min~30min, and then cooling to room temperature, with a heating rate of 50°C / min~200°C / min, a cooling rate of 50°C / min~400°C / min, and maintaining a pressure of 20MPa~80MPa during the sintering process.

6. A high strength, toughness and hardness (TiZrVNb) C according to claim 1. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The sintering method described in step three is hot pressing sintering.

7. A high strength, toughness and hardness (TiZrVNb) C according to claim 6. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The hot pressing sintering process described in step three is: heating from room temperature to 1800℃~2300℃, keeping at 1800℃~2300℃ for 5min~120min, then cooling to room temperature, with a heating rate of 5℃ / min~30℃ / min, a cooling rate of 5℃ / min~50℃ / min, and maintaining a pressure of 20MPa~100MPa during sintering.

8. A high strength, toughness and hardness (TiZrVNb) C according to claim 1 x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that During the sintering process described in step 3, an inert gas needs to be continuously introduced to form a protective atmosphere, or a vacuum state needs to be maintained.

9. A high strength, toughness and hardness (TiZrVNb) C according to claim 8. x A method for preparing a multi-phase multi-component carbide ceramic material, characterized in that The inert gas is argon, helium or krypton, and the vacuum state is <15Pa.