A kind of high temperature resistant glue and its preparation method and application
By using epoxy resin, isocyanate, NH2-MIL(Fe) and hyperbranched polyester graft to modify MoS2, the problem of insufficient bonding ability and mechanical properties of existing glues in high temperature environments is solved, and the problem of insufficient bonding ability and mechanical properties of existing glues in high temperature environments is achieved. Efficient bonding to semiconductors and automotive products.
Patent Information
- Application Number
- CN202410189468.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-20
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-02-20
AI Technical Summary
The existing glue has insufficient bonding capacity and mechanical properties in high-temperature environments, making it difficult to meet the high-temperature application needs of semiconductors and automotive products.
Epoxy resin, isocyanate, NH2-MIL(Fe) and hyperbranched polyester graft modification MoS2 is used as the main raw materials, and high-temperature resistant glue is prepared through hydrothermal reaction and ultrasonic dispersion to enhance its adhesive properties and mechanical properties.
It significantly improves the high temperature resistance and mechanical properties of the glue, and is suitable for bonding applications of semiconductors and automotive products, extending its service life.
Smart Images

Figure BDA0004707257810000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of adhesives, and more specifically, relates to a high temperature resistant glue and a preparation method and application thereof. Background Art
[0002] Adhesives are generally divided into two categories: organic adhesives and inorganic adhesives. Organic adhesives have good viscosity, good flexibility after curing, and are easy to use and process. They are significantly better than inorganic adhesives, so they have been widely used in many fields.
[0003] CN114958273A discloses a flame retardant and high temperature resistant environmentally friendly glue and its preparation method, belonging to the technical field of adhesive materials. The environmentally friendly glue, in parts by weight, includes the following raw materials: isocyanate: 70 parts to 110 parts, polyester polyol: 20 parts to 30 parts, polyether polyol: 15 parts to 25 parts, flame retardant and high temperature resistant additives: 10 parts to 18 parts, epoxy soybean oil: 1 part to 8 parts, organic bismuth catalyst: 0.01 parts to 0.05 parts; the flame retardant and high temperature resistant additives include aluminum hydroxide, magnesium hydroxide, tricresyl phosphate, montmorillonite powder, liquid chlorinated paraffin; the mass ratio of the aluminum hydroxide, the magnesium hydroxide, the tricresyl phosphate, the montmorillonite powder, and the liquid chlorinated paraffin is 8:5:3:7:4. After testing, it has good flame retardant and high temperature resistant properties, and the viscosity and bonding strength are significantly improved, and the product meets environmental protection requirements.
[0004] CN115746759A discloses a high temperature resistant, shock resistant and anti-corrosion structural glue and its preparation method and application. The structural glue is composed of the following raw materials in parts by weight: 25-35 parts of phenolic resin, 18-20 parts of polyurethane resin, 16-18 parts of stearamide, 21-25 parts of curing anti-corrosion agent, 11-15 parts of flame retardant, and 9-11 parts of leveling agent. The high temperature resistant, shock resistant and anti-corrosion coating can have a long shelf life, convenient construction, strong and durable, high bonding strength, a wide range of bonding materials, water resistance, high corrosion resistance, high alkali resistance, high hardness, and high temperature resistance. The high temperature resistant, shock resistant and anti-corrosion structural glue of the present invention has a simple preparation process and is an ideal anti-corrosion coating, which is worthy of industrial promotion. Its temperature resistance can reach more than 100°C, is not easy to melt, and better reduces the wear of the heated surface by the high temperature airflow, reduces the high temperature corrosion rate, prolongs the service life of the substrate, and is conducive to practical use.
[0005] CN117126610A discloses a high temperature resistant vehicle-mounted OCA optical glue, comprising the following components in parts by weight: 80-150 parts of acrylate prepolymer, 0.02-0.08 parts of a first photoinitiator, 0.02-0.05 parts of an inhibitor, 0.01-0.06 parts of a leveling agent, 0.02-0.08 parts of a defoamer, 0.1-0.3 parts of a coupling agent, 0.1-0.3 parts of a cross-linking agent, and 0.03 parts of a first molecular weight regulator; the acrylate prepolymer comprises the following components in parts by weight: 60-85 parts of isooctyl acrylate, 10-15 parts of 2-hydroxyethyl acrylate, 5-15 parts of isobornyl acrylate, 46 parts of acryloylmorpholine, 3-8 parts of dimethylpropionamide, 0.02-0.05 parts of a second photoinitiator, and 0.02-0.05 parts of a second molecular weight regulator. The present invention can effectively improve the tolerance of vehicle-mounted OCA glue in high temperature environments by adjusting the OCA glue formula, so that it can adapt to more extreme thermal conditions, such as extremely hot climates or high-temperature engine compartment interiors.
[0006] Due to different compositions, the areas of use and bonding strength of glue vary. For semiconductors, etc., the glue needs to have good bonding ability, mechanical properties, and a certain degree of high temperature resistance. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a high temperature resistant glue and its preparation method and application. The high temperature resistant glue provided by the present invention comprises the following raw materials: 100 parts of epoxy resin, 6 to 10 parts of isocyanate, 10 to 18 parts of NH2-MIL (Fe), 1 to 5 parts of hyperbranched polyester grafted modified MoS2, 20-30 parts of curing agent, and 280 to 320 parts of acetone. By adding NH2-MIL (Fe) and hyperbranched polyester grafted modified MoS2, the present invention makes the glue have good bonding properties, mechanical properties and good high temperature resistance.
[0008] The purpose of the invention is to provide a high temperature resistant glue.
[0009] Another object of the present invention is to provide a method for preparing the high temperature resistant glue.
[0010] Another object of the present invention is to provide an application of high temperature resistant glue.
[0011] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0012] A high temperature resistant glue, comprising the following raw materials in parts by weight:
[0013] 100 parts of epoxy resin, 6-10 parts of isocyanate, 10-18 parts of NH2-MIL(Fe), 1-5 parts of hyperbranched polyester graft-modified MoS2, 20-30 parts of curing agent, and 280-320 parts of acetone.
[0014] Preferably, the isocyanate is hexamethylene diisocyanate or diphenylmethane-4,4'-diisocyanate; and the curing agent is adipic acid dihydrazide or methylhexahydrophthalic anhydride.
[0015] A further preferred technical solution is that the preparation method of NH2-MIL(Fe) comprises the following steps: dissolving ferric chloride and 2-aminoterephthalic acid in DMF, performing a hydrothermal reaction, then cooling to room temperature, centrifuging, washing, and drying to obtain NH2-MIL(Fe).
[0016] Preferably, the hydrothermal reaction is a hydrothermal reaction at 120-140° C. for 20-40 h; the drying is drying at 80-120° C. for 6-12 h; and the molar ratio of ferric chloride to 2-aminoterephthalic acid is 1:1.5-2.5.
[0017] A further preferred technical solution is that the preparation method of the hyperbranched polyester grafted modified MoS2 comprises the following steps:
[0018] (1) Preparation of MoS2 nanosheets: Sodium molybdate, oxalic acid and thiourea are mixed and ultrasonically dispersed in deionized water. After hydrothermal reaction, the product is washed and dried to obtain MoS2 nanosheets.
[0019] (2) Carboxylation of MoS2 nanosheets: MoS2 nanosheets are ultrasonically dispersed in deionized water, and then bromoacetic acid is added, stirred at 40-60°C for 15-25h, filtered, washed, and dried at 80°C for 10-14h to obtain carboxyl-modified MoS2 nanosheets;
[0020] (3) Ultrasonic dispersion of the terminal hydroxyl hyperbranched polyester and the carboxyl-modified MoS2 nanosheets prepared in step (2) in an appropriate amount of DMF, heating to 50-70°C and continuing ultrasonic dispersion for 1-2 hours, then heating to 110-130°C, stirring and reacting for 20-30 hours. After the reaction is completed, washing with acetone to obtain hyperbranched polyester grafted modified MoS2.
[0021] Preferably, in step (1), the molar ratio of sodium molybdate, oxalic acid and thiourea is 1:1.5:4.8; the hydrothermal condition is 160-200°C for reaction for 16-26h, and the drying is drying at 80°C to constant weight.
[0022] Preferably, in step (2), the molar ratio of the MoS2 nanosheets to bromoacetic acid is 1:11-12; in step (3), the mass ratio of the terminal hydroxyl hyperbranched polyester to the carboxyl-modified MoS2 nanosheets prepared in step (2) is 5-7:1; the terminal hydroxyl hyperbranched polyester is at least one of Hyper H202, Hyper H203, and Hyper H204.
[0023] Based on the above-mentioned method for preparing a high temperature resistant glue, the preparation method includes the following steps: after fully mixing epoxy resin, isocyanate, NH2-MIL (Fe), hyperbranched polyester grafted modified MoS2, and acetone, react at 50-70°C for 4-8 hours; cool to room temperature, add a curing agent, and fully mix to obtain a modified epoxy adhesive.
[0024] The high temperature resistant glue described above is applied to the bonding of semiconductors, electronics or automotive products.
[0025] The present invention has the following beneficial effects:
[0026] (1) The present invention grafts MoS2 with hyperbranched polyester to make it have better dispersibility in the system. At the same time, it forms chemical bonds with the base composite material through hydrogen bonds, so that the high temperature resistance and mechanical properties of the glue are significantly improved.
[0027] (2) By adding NH2-MIL(Fe), the presence of amino groups promotes its dispersion and chemical bonding with the substrate, thereby improving the mechanical properties and high temperature resistance of the glue.
[0028] (3) The glue preparation process of the present invention is simple, the raw material source is abundant, and the application prospect is good. DETAILED DESCRIPTION
[0029] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0030] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0031] Example 1
[0032] A high temperature resistant glue, comprising the following raw materials in parts by weight:
[0033] 100 parts of epoxy resin E42, 8 parts of isocyanate, 14 parts of NH2-MIL(Fe), 3 parts of hyperbranched polyester grafted modified MoS2, 25 parts of curing agent, and 300 parts of acetone; the isocyanate is diphenylmethane-4,4'-diisocyanate; the curing agent is methylhexahydrophthalic anhydride;
[0034] The preparation method of NH2-MIL(Fe) comprises the following steps: dissolving 1 mol of ferric chloride and 2 mol of 2-aminoterephthalic acid in an appropriate amount of DMF, hydrothermally reacting at 120°C for 30 hours, cooling to room temperature, centrifuging, washing, and drying at 100°C for 10 hours to obtain NH2-MIL(Fe).
[0035] The preparation method of hyperbranched polyester grafted modified MoS2 comprises the following steps:
[0036] (1) Preparation of MoS2 nanosheets: 1 mol sodium molybdate, 1.5 mol oxalic acid and 4.8 mol thiourea were mixed and ultrasonically dispersed in 250 mL deionized water and subjected to hydrothermal reaction at 180 °C for 20 h. The product was washed and dried at 80 °C to constant weight to obtain MoS2 nanosheets.
[0037] (2) Carboxylation of MoS2 nanosheets: 1 mol of MoS2 nanosheets was ultrasonically dispersed in 150 mL of deionized water, and then 11.5 mol of bromoacetic acid was added, stirred at 50 °C for 20 h, filtered, washed, and dried at 80 °C for 12 h to obtain carboxyl-modified MoS2 nanosheets;
[0038] (3) Ultrasonic dispersion of 60 g Hyper H203 and 10 g of the carboxyl-modified MoS2 nanosheets prepared in step (2) into an appropriate amount of DMF, heating to 60°C and continuing ultrasonic dispersion for 1.5 h, then heating to 120°C and stirring for 26 h. After the reaction is completed, washing with acetone to obtain hyperbranched polyester-grafted MoS2.
[0039] A method for preparing a high temperature resistant glue; epoxy resin, isocyanate, NH2-MIL(Fe), hyperbranched polyester grafted modified MoS2, and acetone are fully mixed, and reacted at 60°C for 6 hours; the mixture is cooled to room temperature, a curing agent is added, and the mixture is fully mixed to obtain a modified epoxy adhesive.
[0040] Example 2
[0041] A high temperature resistant glue, comprising the following raw materials in parts by weight:
[0042] 100 parts of epoxy resin E42, 10 parts of isocyanate, 10 parts of NH2-MIL(Fe), 5 parts of hyperbranched polyester grafted modified MoS2, 20 parts of curing agent, 320 parts of acetone; the isocyanate is hexamethylene diisocyanate; the curing agent is adipic acid dihydrazide;
[0043] The preparation method of NH2-MIL(Fe) comprises the following steps: dissolving 1 mol of ferric chloride and 2.5 mol of 2-aminoterephthalic acid in an appropriate amount of DMF, hydrothermally reacting at 140° C. for 20 h, then cooling to room temperature, centrifuging, washing, and drying at 120° C. for 6 h to obtain NH2-MIL(Fe).
[0044] The preparation method of hyperbranched polyester grafted modified MoS2 comprises the following steps:
[0045] (1) Preparation of MoS2 nanosheets: The same as the preparation of MoS2 nanosheets in step (1) in Example 1.
[0046] (2) Carboxylation of MoS2 nanosheets: 1 mol of MoS2 nanosheets was ultrasonically dispersed in 150 mL of deionized water, and then 12 mol of bromoacetic acid was added, stirred at 60 °C for 15 h, filtered, washed, and dried at 80 °C for 14 h to obtain carboxyl-modified MoS2 nanosheets;
[0047] (3) Ultrasonic dispersion of 70 g Hyper H204 and 10 g of the carboxyl-modified MoS2 nanosheets prepared in step (2) into an appropriate amount of DMF, heating to 70°C and continuing ultrasonic dispersion for 1 h, then heating to 130°C and stirring for 20 h. After the reaction is completed, washing with acetone to obtain hyperbranched polyester-grafted MoS2.
[0048] A method for preparing a high temperature resistant glue; epoxy resin, isocyanate, NH2-MIL(Fe), hyperbranched polyester grafted modified MoS2, and acetone are fully mixed, and reacted at 70°C for 4 hours; the mixture is cooled to room temperature, a curing agent is added, and the mixture is fully mixed to obtain a modified epoxy adhesive.
[0049] Example 3
[0050] A high temperature resistant glue, comprising the following raw materials in parts by weight:
[0051] 100 parts of epoxy resin E42, 6 parts of isocyanate, 18 parts of NH2-MIL(Fe), 1 part of hyperbranched polyester grafted modified MoS2, 30 parts of curing agent, 280 parts of acetone; the isocyanate is hexamethylene diisocyanate; the curing agent is methylhexahydrophthalic anhydride;
[0052] The preparation method of NH2-MIL(Fe) comprises the following steps: dissolving 1 mol of ferric chloride and 1.5 mol of 2-aminoterephthalic acid in an appropriate amount of DMF, hydrothermally reacting at 120° C. for 40 hours, then cooling to room temperature, centrifuging, washing, and drying at 80° C. for 12 hours to obtain NH2-MIL(Fe).
[0053] The preparation method of hyperbranched polyester grafted modified MoS2 comprises the following steps:
[0054] (1) Preparation of MoS2 nanosheets: The same as the preparation of MoS2 nanosheets in step (1) in Example 1.
[0055] (2) Carboxylation of MoS2 nanosheets: 1 mol of MoS2 nanosheets was ultrasonically dispersed in 150 mL of deionized water, and then 11 mol of bromoacetic acid was added, stirred at 40 °C for 25 h, filtered, washed, and dried at 80 °C for 10 h to obtain carboxyl-modified MoS2 nanosheets;
[0056] (3) Ultrasonic dispersion of 50 g of Hyper H202 and 10 g of the carboxyl-modified MoS2 nanosheets prepared in step (2) into an appropriate amount of DMF, heating to 50°C and continuing ultrasonic dispersion for 2 h, then heating to 110°C and stirring for 30 h. After the reaction is completed, washing with acetone to obtain hyperbranched polyester-grafted MoS2.
[0057] A method for preparing a high temperature resistant glue; epoxy resin, isocyanate, NH2-MIL(Fe), hyperbranched polyester grafted modified MoS2, and acetone are fully mixed, and reacted at 50°C for 8 hours; the temperature is cooled to room temperature, a curing agent is added, and the mixture is fully mixed to obtain a modified epoxy adhesive.
[0058] Example 5
[0059] Except for the difference, the other steps and conditions are exactly the same as those in the embodiment. The difference is that the terminal hydroxyl hyperbranched polyester is Hyper H202.
[0060] Example 6
[0061] Except for the difference, the other steps and conditions are exactly the same as those in the embodiment. The difference is that the terminal hydroxyl hyperbranched polyester is Hyper H204.
[0062] Comparative Example 1
[0063] Comparative Example 1 is compared with Example 1, except that the MoS2 is not grafted with a hyperbranched polyester, and the preparation method of MoS2 is as follows:
[0064] (1) Preparation of MoS2 nanosheets: 1 mol sodium molybdate, 1.5 mol oxalic acid and 4.8 mol thiourea were mixed and ultrasonically dispersed in 250 mL deionized water and subjected to hydrothermal reaction at 180 °C for 20 h. The product was washed and dried at 80 °C to constant weight to obtain MoS2 nanosheets.
[0065] (2) Carboxylation of MoS2 nanosheets: 1 mol of MoS2 nanosheets was ultrasonically dispersed in 150 mL of deionized water, and then 11.5 mol of bromoacetic acid was added, stirred at 50 °C for 20 h, filtered, washed, and dried at 80 °C for 12 h to obtain carboxyl-modified MoS2 nanosheets.
[0066] Comparative Example 2
[0067] Compared with Example 1, Comparative Example 2 differs in that it does not contain NH2-MIL(Fe), and the amount of hyperbranched polyester grafted modified MoS2 is 17 parts.
[0068] Comparative Example 3
[0069] Compared with Example 1, Comparative Example 3 differs in that: 17 parts of NH2-MIL(Fe) are used, and hyperbranched polyester grafted modified MoS2 is not contained.
[0070] Comparative Example 4
[0071] Comparative Example 4 is different from Example 1 in that an equal amount of MIL(Fe) is used instead of NH2-MIL(Fe), wherein the preparation method of MIL(Fe) is as follows: 1 mol of ferric chloride and 2 mol of terephthalic acid are dissolved in an appropriate amount of DMF, and the mixture is hydrothermally reacted at 120°C for 30 hours, then cooled to room temperature, centrifuged, washed, and dried at 100°C for 10 hours to obtain MIL(Fe).
[0072] The performance of test examples 1-5 and comparative example 14:
[0073] Tensile strength: Tested in accordance with GB / T 528-1998;
[0074] Shear strength: Tested in accordance with GB / T 7124-1986;
[0075] (1) The epoxy adhesives obtained in the embodiments and comparative examples were coated on PCB boards (100 mm × 25 mm × 2 mm), respectively, and pressed with PCB sheets. The thickness of the adhesive layer was controlled by a 0.13 mm copper wire. The adhesive layer area was 25 mm × 4.8 mm. The adhesive was heated and cured at 128° C. for 4 h to prepare experimental sheets. The tensile strength and shear strength were tested at room temperature. The test results are shown in Table 1.
[0076] (2) Test piece A was prepared according to the room temperature test, and test piece A was heat-cured in an oven at 300°C for 30 minutes to produce test piece B; the retention rate of tensile strength and shear strength of test piece B under high temperature was tested. The test results are shown in Table 1.
[0077] Table 1:
[0078]
[0079] It can be seen from Table 1 that the MoS2 of the present invention can significantly improve the mechanical properties and high temperature resistance of the glue by being grafted with hyperbranched polyester. By adding NH2-MIL(Fe), the mechanical properties and high temperature resistance of the glue are significantly improved due to the presence of amino groups.
[0080] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A high temperature resistant glue, characterized in that: The composition comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 6-10 parts of isocyanate, 10-18 parts of NH2-MIL (Fe), 1-5 parts of hyperbranched polyester grafted modified MoS2, 20-30 parts of curing agent, and 280-320 parts of acetone; the preparation method of NH2-MIL (Fe) comprises the following steps: dissolving ferric chloride and 2-aminoterephthalic acid in DMF, hydrothermal reaction, cooling to room temperature, centrifuging, washing, and drying to obtain NH2-MIL (Fe); the hydrothermal reaction is a hydrothermal reaction at 120-140° C. for 20-40 hours; the drying is drying at 80-120° C. for 6-12 hours; the molar ratio of ferric chloride to 2-aminoterephthalic acid is 1:1.5-2.5; The preparation method of the hyperbranched polyester grafted modified MoS2 comprises the following steps: (1) Preparation of MoS2 nanosheets: Sodium molybdate, oxalic acid and thiourea are mixed and ultrasonically dispersed in deionized water. After hydrothermal reaction, the product is washed and dried to obtain MoS2 nanosheets. The molar ratio of sodium molybdate, oxalic acid and thiourea is 1:1.5:4.
8. The hydrothermal conditions are 160-200°C for reaction for 16-26h, and the drying is performed at 80°C until constant weight. (2) Carboxylation of MoS2 nanosheets: ultrasonically dispersing the MoS2 nanosheets in deionized water, then adding bromoacetic acid, stirring at 40-60°C for 15-25h, filtering, washing, and drying at 80°C for 10-14h to obtain carboxyl-modified MoS2 nanosheets; the molar ratio of the MoS2 nanosheets to bromoacetic acid is 1:11-12; (3) Ultrasonic dispersion of the terminal hydroxyl hyperbranched polyester and the carboxyl-modified MoS2 nanosheets prepared in step (2) in an appropriate amount of DMF, heating to 50-70°C and continuing ultrasonic dispersion for 1-2 hours, then heating to 110-130°C and stirring for reaction for 20-30 hours. After the reaction is completed, washing with acetone to obtain hyperbranched polyester grafted MoS2; the mass ratio of the terminal hydroxyl hyperbranched polyester and the carboxyl-modified MoS2 nanosheets prepared in step (2) is 5-7:1; the terminal hydroxyl hyperbranched polyester is at least one of Hyper H202, Hyper H203, and Hyper H204.
2. The high temperature resistant glue according to claim 1, characterized in that: The isocyanate is hexamethylene diisocyanate or diphenylmethane-4,4'-diisocyanate; and the curing agent is adipic acid dihydrazide or methylhexahydrophthalic anhydride.
3. A method for preparing a high temperature resistant glue according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: fully mixing epoxy resin, isocyanate, NH2-MIL (Fe), hyperbranched polyester grafted modified MoS2 and acetone, reacting at 50-70°C for 4-8 hours; cooling to room temperature, adding a curing agent and fully mixing to obtain a modified epoxy adhesive.
4. The high temperature resistant glue according to claim 3 is applied to the bonding of semiconductor, electronic or automotive products.