A method for preparing porous nitrogen-doped carbon in-situ electrode

By introducing porous nitrogen-doped structure and cobalt salt into the carbon in situ electrode, combined with electroactive monomers, the problem of low ORR performance is solved, and an efficient non-metal-based catalyst is achieved, reducing costs and improving electrocatalytic performance is improved. .

CN118099458BActive Publication Date: 2024-11-22LUOYANG NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410065190.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2024-11-22
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

In the prior art, oxygen reduction reaction (ORR) is slow in zinc-empty batteries, resulting in the need of efficient precious metal-based catalysts, but their high cost and scarcity limit large-scale applications, and finding non-metal-based catalysts to improve ORR performance has become an urgent need. .

Method used

The preparation method of porous nitrogen-doped carbon in situ electrode is adopted to provide a source of N impurity through dopamine, and the nitrogen and hydrogen elements produced by its decomposition are used to make pores on the carbon framework, and metal cobalt and electroactive monomers are introduced to form high Active sites to enhance electrocatalytic performance.

Benefits of technology

The performance of oxygen reduction reaction has been successfully improved, the use of precious metals has been eliminated, the production cost has been reduced, and the process has been simple, the operation is convenient, and the equipment conditions are low, which has achieved the efficient application of non-metal-based electrocatalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118099458B_ABST
    Figure CN118099458B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a porous nitrogen-doped carbon in-situ electrode, comprising the following steps: S1. preparing a PDA / CC precursor; S2. preparing a Co / PDA / CC precursor; S3. surface modification of the Co / PDA / CC precursor; S4. preparing a P-NC in-situ electrode. The invention uses dopamine (PDA) to provide an N impurity source, which is doped into a carbon material skeleton that is gradually formed subsequently, and simultaneously uses nitrogen, hydrogen and other elements generated by decomposition to form pores on the carbon skeleton and assist in reducing the generated metal cobalt and electroactive monomers to enter the pores, thereby improving the electrocatalytic performance of the electrode while preventing the porous carbon structure from collapsing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrode material preparation, and in particular to a method for preparing a porous nitrogen-doped carbon in-situ electrode. Background Art

[0002] Due to the increasingly serious global environmental problems caused by the burning of fossil fuels, new energy conversion materials using clean and renewable resources have received increasing attention in recent years. In zinc-air batteries, OER and ORR reactions are involved. Since the oxygen reduction reaction (ORR) is slow, it is necessary to develop highly active catalysts to reduce the reaction energy barrier. So far, the most efficient electrocatalysts are still precious metal-based catalysts, but their high prices and scarce resources have greatly limited their large-scale application. It has become particularly important to find non-metal-based catalysts to improve ORR performance.

[0003] According to the literature survey, Dai reported that nitrogen-doped carbon nanotube arrays exhibited high ORR electrocatalytic activity in alkaline media, even better than Pt (Science 2009, 323, 760.). This discovery triggered the research field of carbon-based metal-free ORR electrocatalysts. Since then, great progress has been made in carbon-based nanomaterials and the understanding of the interesting ORR process, which has promoted the research of transition metal-based ORR electrocatalysts.

[0004] Therefore, it is an urgent problem to be solved at present to provide a new non-metal catalyst to improve ORR performance through carbon-based nanomaterials. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a porous nitrogen-doped carbon in-situ electrode. The present invention uses dopamine (PDA) to provide a N impurity source, which is doped into the carbon material skeleton that is gradually formed subsequently. At the same time, the nitrogen, hydrogen and other elements generated by its decomposition are used to form pores on the carbon skeleton and assist in the reduction of the generated metal cobalt and the electroactive monomers to enter the pores, thereby improving the electrocatalytic performance of the electrode while preventing the porous carbon structure from collapsing.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a porous nitrogen-doped carbon in-situ electrode comprises the following steps:

[0008] S1. Preparation of PDA / CC precursor: preparing a Tris solution with a pH range of 8-9, dissolving dopamine hydrochloride in the solution, completely immersing the carbon cloth and hanging it in the mixed solution to allow it to stand, attaching PDA on the surface of the carbon cloth, and obtaining a PDA / CC material;

[0009] S2. Preparation of Co / PDA / CC precursor: soaking PDA / CC in a cobalt acetate aqueous solution for 0.5-1 h to attach cobalt salt to obtain Co / PDA / CC material;

[0010] S3. Surface modification of Co / PDA / CC precursor:

[0011] S301. The Co / PDA / CC material prepared in S2 is re-immersed in the mixed solution of step S1 and allowed to stand to adhere to the surface of the Co / PDA / CC material;

[0012] S302. Dispersing the Co / PDA / CC material treated in S301 and the electroactive monomer in methanol, adding a crosslinking agent and an initiator, and stirring for 1-2 hours to obtain a surface-modified Co / PDA / CC material;

[0013] S4. Preparation of P-NC in-situ electrode: The Co / PDA / CC material prepared in step S302 is treated by CVD method under argon atmosphere, and then pickled to obtain a P-NC in-situ electrode.

[0014] Preferably, in S1, the concentration of dopamine hydrochloride is 0.2-1.2 mg / mL, and the standing time is 20-28 h.

[0015] Preferably, in S2, the concentration of cobalt acetate is 200-1200 mM.

[0016] Preferably, in S301, the standing time is 20-22 hours.

[0017] Preferably, in S302, the mass ratio of the Co / PDA / CC material to the electroactive monomer is 1:3-4.

[0018] Preferably, the electroactive monomer is selected from one or more of aniline, pyrrole and thiophene.

[0019] Preferably, the cross-linking agent is selected from one or more of thioether, tertiary amine and tert-butyl peroxide.

[0020] Preferably, the initiator is selected from one or more of ammonium persulfate, anisole peroxide, and nitrosamine compounds.

[0021] Preferably, in S4, the parameters of the CVD method are set as follows: heating to 350-400°C at a heating rate of 10°C / min, keeping warm for 1-2h, then heating to 850-900°C at a heating rate of 5°C / min, keeping warm for 2-3h.

[0022] Preferably, in S4, the pickling is performed using a 0.5-1M H2SO4 solution at a temperature of 80-90°C for 12-15 hours.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The P-NC in-situ electrode prepared by the present invention has abundant active sites and can effectively enhance the ORR performance of the material;

[0025] 2. The present invention successfully uses carbon-based nanomaterials to prepare non-metal-based electrocatalysts. Compared with precious metal-based catalysts, the present invention eliminates the use of precious metals, greatly reduces production costs, and improves economic benefits;

[0026] 3. The process of the present invention is simple, easy to operate, and has low requirements on equipment conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flow chart of the preparation process of the porous nitrogen-doped carbon in-situ electrode;

[0028] Figure 2 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 1, and (b) is the C plotted from (a). dl curve;

[0029] Figure 3 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 2, and (b) is the C plotted from (a). dl curve;

[0030] Figure 4 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 3, and (b) is the C plotted from (a). dl curve;

[0031] Figure 5 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 4, and (b) is the C plotted from (a). dl curve;

[0032] Figure 6 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 5, and (b) is the C plotted from (a). dl curve;

[0033] Figure 7 The performance test diagrams of the porous nitrogen-doped carbon in-situ electrode of the present invention are as follows: (a) is the variable speed CV diagram of the sample prepared in Example 6, and (b) is the C plotted from (a).dl curve;

[0034] Figure 8 The SEM scanning images of Example 2: (a) is a low-magnification SEM of Example 2, and (b) is a high-magnification SEM of Example 2;

[0035] Fig. 9 The SEM scanning images of Example 4: (a) is a low-magnification SEM of Example 4, and (b) is a high-magnification SEM of Example 4;

[0036] Fig.10 The SEM scanning images of Example 6: (a) is a low-magnification SEM of Example 6, and (b) is a high-magnification SEM of Example 6;

[0037] Fig.11 The SEM scanning images of Example 7: (a) is a low-magnification SEM of Example 7, and (b) is a high-magnification SEM of Example 7;

[0038] Fig.12 These are SEM scanning images of Example 8: (a) is a low-magnification SEM of Example 8, and (b) is a high-magnification SEM of Example 8. DETAILED DESCRIPTION

[0039] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] See also Figure 1-12 , the present invention provides a technical solution:

[0041] Embodiment 1:

[0042] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0043] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.02 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.02 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.25 g of aniline in 20 ml of methanol, add 0.15 g of thioether and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 1.

[0044] Embodiment 2:

[0045] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0046] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.04 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.04 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.25 g of pyrrole in 20 ml of methanol, add 0.15 g of thioether and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 2.

[0047] Embodiment 3:

[0048] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0049] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.06 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.06 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with re-attached PDA and 1.3 g of thiophene in 20 ml of methanol, add 0.20 g of tertiary amine and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 3.

[0050] Embodiment 4:

[0051] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0052] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.25 g of pyrrole in 20 ml of methanol, add 0.17 g of thioether and 0.18 g of anisole peroxide, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 4.

[0053] Embodiment 5:

[0054] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0055] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.1 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.1 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.27 g of aniline in 20 ml of methanol, add 0.15 g of thioether and 0.18 g of anisole peroxide, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 5.

[0056] Embodiment 6:

[0057] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0058] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.12 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 800 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.12 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.25 g of thiophene in 20 ml of methanol, add 0.16 g of thioether and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tube furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 6.

[0059] Embodiment 7:

[0060] A method for preparing a porous nitrogen-doped carbon in-situ electrode:

[0061] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse the carbon cloth (CC) in the mixture and suspend it, and leave it for 24 hours to attach PDA. Soak PDA / CC in 400 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse the Co / PDA / CC material in the mixture and suspend it, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.25 g of pyrrole in 20 ml of methanol, add 0.15 g of tertiary amine and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tube furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 7.

[0062] Embodiment 8:

[0063] Prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse and suspend the carbon cloth (CC) in the mixture, and leave it for 24 hours to attach PDA. Soak PDA / CC in a 1200 mM cobalt acetate solution for half an hour to attach cobalt salt. Re-prepare 100 mL of Tris solution with a pH of 8.5, dissolve 0.08 g of dopamine hydrochloride in it, completely immerse and suspend the Co / PDA / CC material in the mixture, and leave it for 24 hours to attach PDA. Disperse the Co / PDA / CC material with reattached PDA and 1.20 g of aniline in 20 ml of methanol, add 0.17 g of thioether and 0.18 g of ammonium persulfate, and stir for 1 hour. The temperature was raised to 350°C at a heating rate of 10°C / min in an argon atmosphere using a tubular furnace, and kept at that temperature for 1 hour, and then raised to 850°C at a heating rate of 5°C / min, and kept at that temperature for 2 hours to obtain P-NC. It was then placed at 80°C for a 0.5M H2SO4 pickling treatment, and dried to obtain the sample of Example 8.

[0064] Performance testing:

[0065] 1. Characterization conditions

[0066] The CV test method in the embodiment of the invention is: the prepared sample is used as the working electrode, the carbon rod is used as the counter electrode, and the saturated Hg / HgO electrode is used as the reference electrode. The electrolyte used is: 0.1M KOH aqueous solution, and the scanning speed is 20-100mV / s. The solution is saturated with oxygen before the CV test. The saturated Hg / HgO electrode is calibrated with a reversible hydrogen electrode, and the potentials described below are all potentials relative to the reversible hydrogen electrode. The CV test was tested using the Shanghai Chenhua workstation. Scanning electron microscope (SEM) images were obtained using an Inspect F50 scanning electron microscope (FEI America).

[0067] 2. Characterization Data Analysis

[0068] Figure 2 (a) is the variable speed CV diagram of the sample prepared in Example 1, and (b) is the C curve obtained by plotting the C curve from (a). dl Curve. Measured C dl The value is 22.67mF cm -2 , the ECSA value is 566.75.

[0069] Figure 3 (a) is the variable speed CV graph of the sample prepared in Example 2, and (b) is the Cdl curve drawn from (a). dl The value is 24.6mF cm -2 , the ECSA value is 615.

[0070] Figure 4 (a) is the variable speed CV diagram of the sample prepared in Example 3, and (b) is the C curve obtained by plotting the curve in (a). dl Curve. Measured C dl The value is 19.74mF cm -2 , the ECSA value is 493.5.

[0071] Figure 5 (a) is the variable speed CV diagram of the sample prepared in Example 4, and (b) is the C curve obtained by plotting the curve in (a). dl Curve. Measured C dl The value is 20.22mF cm -2 , the ECSA value is 505.5.

[0072] Figure 6 (a) is the speed CV diagram of the sample prepared in Example 5, and (b) is the C curve obtained by plotting the C curve from (a). dl Curve. Measured C dl The value is 17.54mF cm -2 , the ECSA value is 438.5.

[0073] Figure 7(a) is the speed CV diagram of the sample prepared in Example 6, and (b) is the C curve obtained by plotting the curve in (a). dl Curve. Measured C dl The value is 15.33mF cm -2 , the ECSA value is 383.25.

[0074] Figure 8 (a) is a low-magnification SEM of Example 2, and (b) is a high-magnification SEM of Example 2. It can be observed that nitrogen-doped carbon grows on the surface of the carbon cloth, and there are many holes on the surface.

[0075] Fig. 9 (a) is a low-magnification SEM of Example 4, and (b) is a high-magnification SEM of Example 4. It can be observed that nitrogen-doped carbon grows on the surface of the carbon cloth, and there are many holes on the surface.

[0076] Fig.10 (a) is a low-magnification SEM of Example 6, and (b) is a high-magnification SEM of Example 6. It can be observed that nitrogen-doped carbon grows on the surface of the carbon cloth, and there are many holes on the surface.

[0077] Fig.11 (a) is a low-magnification SEM of Example 7, and (b) is a high-magnification SEM of Example 7. It can be observed that nitrogen-doped carbon grows on the surface of the carbon cloth, and there are many holes on the surface.

[0078] Fig.12 (a) is a low-magnification SEM of Example 8, and (b) is a high-magnification SEM of Example 8. It can be observed that nitrogen-doped carbon grows on the surface of the carbon cloth, and there are many dense holes on the surface.

[0079] The present invention characterizes the performance of Examples 1-8. It can be seen from the SEM scans of Examples 2, 4, 6, 7, and 8 that the present invention successfully creates holes in the carbon cloth on the basis of introducing electroactive monomers and cobalt salts, expands its specific surface area, increases active sites, and grows nitrogen-doped carbon on its surface, which indicates that the present invention successfully prepares the P-NC in-situ electrode. Further, the variable speed CV diagrams of Examples 1-6 and C dl The curve shows that the P-NC in-situ electrode prepared by the present invention has stable working performance at different scanning speeds and has excellent application prospects.

[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a porous nitrogen-doped carbon in-situ electrode, characterized in that: The following steps are involved: S1. Preparation of PDA / CC precursor: preparing a Tris solution with a pH range of 8-9, dissolving dopamine hydrochloride in the solution, completely immersing the carbon cloth and hanging it in the mixed solution to allow it to stand, attaching PDA on the surface of the carbon cloth, and obtaining a PDA / CC material; S2. Preparation of Co / PDA / CC precursor: soaking PDA / CC in a cobalt acetate aqueous solution for 0.5-1 h to attach cobalt salt to obtain Co / PDA / CC material; S3. Surface modification of Co / PDA / CC precursor: S301. The Co / PDA / CC material prepared in S2 is re-immersed in the mixed solution of step S1 and allowed to stand to adhere to the surface of the Co / PDA / CC material; S302. Dispersing the Co / PDA / CC material treated in S301 and the electroactive monomer into methanol, adding a crosslinking agent and an initiator, and stirring for 1-2 hours to obtain a surface-modified Co / PDA / CC material; S4. Preparation of P-NC in-situ electrode: The surface-modified Co / PDA / CC material was treated by heating to 350°C at a heating rate of 10°C / min in an argon atmosphere in a tube furnace, and kept at this temperature for 1 h. The material was then heated to 850°C at a heating rate of 5°C / min, kept at this temperature for 2 h, and then pickled to obtain a P-NC in-situ electrode. The electroactive monomer is selected from one or more of aniline, pyrrole and thiophene.

2. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: In S1, the concentration of dopamine hydrochloride is 0.2-1.2 mg / mL, and the standing time is 20-28 h.

3. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: In S2, the concentration of the cobalt acetate is 200-1200 mM.

4. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: In S301, the standing time is 20-22 hours.

5. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: In S302, the mass ratio of the Co / PDA / CC material to the electroactive monomer is 1:3-4.

6. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: The cross-linking agent is selected from one or more of thioether, tertiary amine and tert-butyl peroxide.

7. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: The initiator is selected from one or more of ammonium persulfate, anisole peroxide, and nitrosamine compounds.

8. The method for preparing a porous nitrogen-doped carbon in-situ electrode according to claim 1, characterized in that: In S4, the pickling is carried out using 0.5-1M H2SO4 solution at a temperature of 80-90°C for 12-15 hours.