Preparation method and application of chitosan modified LATP standard solid electrolyte
Through the preparation of chitosan-modified LATP benchmark solid electrolyte, the problems of irreversible reactivity and poor interface contact of NASICON structure electrolyte in lithium metal batteries are solved, and the electrochemical performance of the electrolyte and the cycle stability of lithium metal batteries are significantly improved. Capacity retention rate.
Patent Information
- Application Number
- CN202410235726.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-01
AI Technical Summary
The existing NASICON structure Li1+xAlxTi2-x(PO4)3 (LATP) solid electrolyte has irreversible reactivity in lithium metal batteries, difficulty in obtaining high relative density and satisfactory Li+ conductivity, and the hard and brittle characteristics of ceramics resulting in solid-solid interface Poor contact problem.
The chitosan-modified LATP benchmark solid-state electrolyte was prepared by coating chitosan on Li1.3Al0.3Ti1.7(PO4)3 nanoparticles and combining it with PVDF-HFP and LiTFSI, and it was prepared by casting method. It produces an electrolyte membrane with a uniform structure and enhances the compatibility and dispersion of fillers and polymer matrix.
Significantly improve the ionic conductivity, lithium ion migration number and electrochemical stability window of the quasi-solid electrolyte, improve the specific discharge capacity and rate performance of lithium metal batteries, extend the service life, and ensure high cycle stability and capacity retention rate .
Smart Images

Figure CN118099540B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a quasi-solid electrolyte. Background Art
[0002] Lithium-ion batteries are currently the dominant power source for consumer electronics, electric vehicles, and grid energy storage. They have a high theoretical capacity (3860mAhg –1 ) and low reduction potential (–3.04 V vs standard hydrogen electrode) are considered to be the ultimate goal of the next generation of battery anodes. Currently, lithium-ion batteries based on organic liquid electrolytes are difficult to support the rapid development of portable electronics and electric vehicles due to their limited energy density and safety issues. Solid-state lithium batteries (SSLBs) replace liquid electrolytes with solid electrolytes (SSEs) and directly use lithium metal anodes. Due to their advantages such as high energy density and high safety, they are considered to be a key energy storage technology with great development prospects. In order to develop SSLBs, it is necessary to explore materials with high ionic conductivity, Li + Transfer number, wide electrochemical stability window and good chemical / electrochemical compatibility with electrodes. + Conductors, including garnet type (Li7La3Zr2O 12 )、NASICON(Li 1.3 Al 0.3 Ti 1.7 (PO4)3) type, perovskite type (Li 0.35 La 0.55 TiO3), thiophosphate type (Li6PS5X (where X = Cl, Br, I)) and sulfide type (Li 10 GeP2S 12 )Li + Conductor. Among them, Li with NASICON structure 1+x Al x Ti 2-x (PO4)3(LATP) has high room temperature Li + Conductivity (10 -4 ~10 -3 Scm -1 ), wide electrochemical stability window, low oxygen moisture sensitivity and low cost, and has been reported to be used in solid-state lithium-ion, Li-S and Li-O2 batteries. However, there are still some obstacles in the practical application of LATP, including: (1) due to the 4+ / Ti 3+ The redox couple, LATP, and the irreversible reactivity of the lithium metal anode; (2) It is difficult to obtain high relative density and meet the requirements of Li +The conductivity of LATP; (3) due to the hard and brittle characteristics of LATP ceramics, the solid-solid interface contact between LATP and the electrode is poor. In order to solve these challenges, a composite solid electrolyte (CSEs) composed of polymer electrolytes, inorganic ceramic electrolyte fillers and some lithium salts was proposed. In CSEs, polymer electrolytes are used to provide soft interface contact and better flexibility with the electrode, while inorganic ceramics are used as fillers to ensure sufficient ionic conductivity and electrochemical stability. Among them, polymer materials such as polyethylene oxide (PEO), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polymethyl methacrylate (PMMA), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) have been widely used as substrates for polymer electrolytes. Among these polymers, PVDF-HFP has the advantages of high dielectric constant, good stability, strong heat resistance and high mechanical strength. It can be used as a flexible polymer matrix to manufacture reliable composite electrolytes and construct high-performance and high-safety lithium metal batteries. In addition, in order to solve the dispersibility problem of ceramic fillers, their surfaces need to be modified to improve direct compatibility with polymers. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a preparation method and application of a chitosan-modified LATP reference solid electrolyte.
[0004] A method for preparing a chitosan-modified LATP reference solid electrolyte is specifically completed by the following steps:
[0005] 1. Preparation of CS@LATP nanoparticles:
[0006] Chitosan was added to a mixed solution of glacial acetic acid and deionized water, and magnetic stirring was performed until the chitosan was completely dissolved. Then Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder was ultrasonicated for a period of time, heated and stirred for a period of time, washed with water several times, and then redispersed in deionized water, heated to 35℃~45℃, and then added with 45%~55% glutaraldehyde solution by mass, stirred continuously for a period of time for cross-linking reaction, and then washed with deionized water and anhydrous ethanol several times in turn, and dried to obtain CS@LATP nanoparticles;
[0007] 2. Preparation of electrolyte:
[0008] CS@LATP nanoparticles were added to N,N-dimethylformamide, ultrasonicated for a period of time, and then PVDF-HFP and LiTFSI were added, heated and magnetically stirred for a period of time to obtain a casting solution; the casting solution was poured on a glass plate with a groove after vacuum degassing, and then placed on a heating plate to dry for a period of time, and finally dried at 70°C to 80°C for a period of time to obtain an electrolyte membrane; the electrolyte membrane was cut into discs to obtain a chitosan-modified LATP benchmark solid electrolyte.
[0009] A chitosan-modified LATP-based solid electrolyte for application in lithium metal batteries.
[0010] Principle of the present invention:
[0011] Chitosan (CS) is a product of the natural polysaccharide chitin with some acetyl groups removed, and has the advantages of biodegradability, biocompatibility, and non-toxicity. Chitosan molecules have a complex double helix structure, contain a large number of hydroxyl groups, amino groups, and N-acetamide groups, and are easy to form a variety of intramolecular and intermolecular hydrogen bonds. In addition, the hydroxyl groups and amino groups in chitosan have coordination and chelation effects, which can provide more active sites and serve as bridges to enhance the compatibility of inorganic fillers and polymer matrices. The present invention spontaneously coats chitosan on Li by solution self-polymerization. 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP) nanoparticles, and a uniformly structured electrolyte membrane is prepared by a casting method; the CS@LATP nanoparticles prepared by the present invention have high mechanical strength and abundant active sites, and enhance the interaction between the filler and the polymer matrix, so that it is easy to disperse evenly in the matrix, avoid agglomeration effect, and can significantly enhance the electrochemical properties of the electrolyte.
[0012] Advantages of the present invention:
[0013] The present invention tests the electrochemical performance of the obtained PVDF-HFP benchmark solid electrolyte. The results show that by introducing CS@LATP nanofiller, the ionic conductivity of the quasi-solid electrolyte is increased from 4.9×10 –5 Scm –1 Significantly increased to 2.6×10 – 4 Scm –1 The lithium ion transfer number is 0.28, the oxidation potential is increased to 5.07V, and the assembled Li|QPE|LiFePO4 full battery has a capacity of 161.9mAhg at a rate of 0.1C. –1 The high discharge capacity is 114.6 mAh g at a rate of 2C. –1The specific capacity shows that the chitosan-modified LATP reference solid electrolyte provided by the present invention has excellent rate performance. The present invention tested the service life of the obtained chitosan-modified LATP reference solid electrolyte. The results showed that after 700 cycles at a rate of 0.5C, it had a capacity retention rate of more than 72.2%, indicating that the chitosan-modified LATP reference solid electrolyte prepared by the present invention has high cycle stability and service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 The SEM and EDX element images of the CS@LATP nanoparticles prepared in step 1 of Example 1;
[0015] Figure 2 The SEM images of the plane and cross section of PH-LATP-Free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, where a, b and c are planes, and d, e and f are cross sections;
[0016] Figure 3 XRD patterns of PH-LATP-free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes;
[0017] Figure 4 a in the figure is the Arrhenius curve of PH-LATP-free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes. Figure 4 b is the lithium ion migration number of PH-CS@LATP-2.5 electrolyte membrane, Figure 4 c in the middle is the electrochemical stability window of PH-CS@LATP-2.5 electrolyte membrane;
[0018] Figure 5 is the limiting current density of PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes;
[0019] Figure 6 The lifespan of symmetric batteries assembled using PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, respectively;
[0020] Figure 7 The rate performance curves of quasi-solid-state batteries assembled using PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, respectively;
[0021] Figure 8 The cycling performance curves of quasi-solid-state batteries assembled using PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes at a rate of 0.5C. DETAILED DESCRIPTION
[0022] Specific implementation method 1: This implementation method is a method for preparing a chitosan-modified LATP reference solid electrolyte, which is specifically completed by the following steps:
[0023] 1. Preparation of CS@LATP nanoparticles:
[0024] Chitosan was added to a mixed solution of glacial acetic acid and deionized water, and magnetic stirring was performed until the chitosan was completely dissolved. Then Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder was ultrasonicated for a period of time, heated and stirred for a period of time, washed with water several times, and then redispersed in deionized water, heated to 35℃~45℃, and then added with 45%~55% glutaraldehyde solution by mass, stirred continuously for a period of time for cross-linking reaction, and then washed with deionized water and anhydrous ethanol several times in turn, and dried to obtain CS@LATP nanoparticles;
[0025] 2. Preparation of electrolyte:
[0026] CS@LATP nanoparticles were added to N,N-dimethylformamide, ultrasonicated for a period of time, and then PVDF-HFP and LiTFSI were added, heated and magnetically stirred for a period of time to obtain a casting solution; the casting solution was poured on a glass plate with a groove after vacuum degassing, and then placed on a heating plate to dry for a period of time, and finally dried at 70°C to 80°C for a period of time to obtain an electrolyte membrane; the electrolyte membrane was cut into discs to obtain a chitosan-modified LATP benchmark solid electrolyte.
[0027] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the volume ratio of glacial acetic acid to deionized water in the mixed solution of glacial acetic acid and deionized water described in step 1 is (2-5):(95-98); the volume ratio of the mass of chitosan described in step 1 to the mixed solution of glacial acetic acid and deionized water is 0.1 g:(95 mL-10 mL). The other steps are the same as those in specific embodiment 1.
[0028] Specific implementation method three: This implementation method is different from specific implementation method one or two in that: the Li in step one 1.3 Al 0.3 Ti 1.7 The mass ratio of (PO4)3 powder to the mixed solution of glacial acetic acid and deionized water is 0.1g:(95mL-100mL); the mass volume ratio of chitosan and glutaraldehyde solution with a mass fraction of 45%-55% described in step 1 to deionized water is 0.1g:(4μL-6μL):100mL. The other steps are the same as those in the first or second embodiment.
[0029] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the ultrasonic time in step 1 is 20 min to 40 min; the heating and stirring temperature in step 1 is 40° C. to 50° C., and the heating and stirring time is 3 h to 5 h; the number of water washings in step 1 is 3 to 5 times. The other steps are the same as those in specific embodiments 1 to 3.
[0030] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the cross-linking reaction time in step 1 is 3h to 5h; deionized water and anhydrous ethanol are used for washing 3 to 5 times respectively in step 1. The other steps are the same as those in specific embodiments 1 to 4.
[0031] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the mass fraction of CS@LATP nanoparticles in the casting solution described in step 2 is 0.5% to 7%; the mass fraction of PVDF-HFP in the casting solution described in step 2 is 15% of N,N-dimethylformamide; the mass ratio of LiTFSI to PVDF-HFP in the casting solution described in step 2 is 1:3. The other steps are the same as specific embodiments 1 to 5.
[0032] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the ultrasonic time in step 2 is 20 min to 30 min; the temperature of the heating magnetic stirring in step 2 is 45°C to 55°C, and the heating magnetic stirring time is 10 h to 12 h; the vacuum degassing time in step 2 is 20 min to 40 min. The other steps are the same as those in specific embodiments 1 to 6.
[0033] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that: in step 2, the electrolyte is placed on a heating plate at a temperature of 35°C to 45°C for 2h to 4h and finally dried at 70°C to 80°C for 10h to 12h; the thickness of the electrolyte membrane in step 2 is 100μm to 140μm; in step 2, the electrolyte membrane is cut into discs with a diameter of 16mm. The other steps are the same as those in specific embodiments 1 to 7.
[0034] Specific implementation method 9: This implementation method is an application of a chitosan-modified LATP standard solid electrolyte in a lithium metal battery.
[0035] Specific embodiment 10: The difference between this embodiment and specific embodiment 9 is that when a chitosan-modified LATP reference solid electrolyte is used in a lithium metal battery, it is transferred to a glove box filled with argon, and 2 μL of lithium battery electrolyte is dripped on both sides of the electrolyte to improve the interface contact between the electrode and the electrolyte; the lithium battery electrolyte is obtained by dissolving LiPF6 in a mixture of EC, DEC and EMC, wherein the volume ratio of EC, DEC and EMC in the mixture is 1:1:1; the concentration of LiPF6 is 1 mol / L. The other steps are the same as those in specific embodiment 9.
[0036] The following examples are used to verify the beneficial effects of the present invention:
[0037] Comparative Example 1: The preparation method of quasi-solid electrolyte (PH-LATP-Free) is specifically completed according to the following steps:
[0038] PVDF-HFP and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were added to N,N-dimethylformamide (DMF), heated at 50°C with magnetic stirring for 12 hours to obtain a casting solution; the casting solution was vacuum degassed and then cast on a glass plate with a groove, and then placed on a heating plate at 40°C for 3 hours, and finally dried at 70°C for 12 hours to obtain an electrolyte membrane with a thickness of 100 μm; the electrolyte membrane was cut into discs with a diameter of 19 mm to obtain a quasi-solid electrolyte (PH-LATP-Free);
[0039] The mass fraction of PVDF-HFP in the casting liquid to N,N-dimethylformamide is 15%;
[0040] The mass ratio of LiTFSI to PVDF-HFP in the casting solution described in step 2 is 1:3.
[0041] Comparative Example 2: The preparation method of LATP reference solid electrolyte (PH-LATP-2.5) is specifically completed according to the following steps:
[0042] Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder (LATP) was added to N,N-dimethylformamide (DMF), ultrasonicated for 20 min, then PVDF-HFP and LiTFSI were added, heated at 50°C with magnetic stirring for 12 h to obtain a casting solution; the casting solution was vacuum degassed and poured on a glass plate with a groove, then placed on a heating plate at 40°C for 3 h, and finally dried at 70°C for 12 h to obtain an electrolyte membrane with a thickness of 100 μm; the electrolyte membrane was cut into discs with a diameter of 19 mm to obtain a LATP benchmark solid electrolyte (PH-LATP-2.5);
[0043] The mass fraction of LATP in the casting liquid is 2.5%;
[0044] The mass fraction of PVDF-HFP in the casting liquid to N,N-dimethylformamide is 15%;
[0045] The mass ratio of LiTFSI to PVDF-HFP in the casting solution is 1:3.
[0046] Example 1: A method for preparing a chitosan-modified LATP reference solid electrolyte (PH-CS@LATP-2.5), which is specifically completed by the following steps:
[0047] 1. Preparation of CS@LATP nanoparticles:
[0048] 0.1 g chitosan was added to a mixed solution of 2 mL acetic acid and 98 mL deionized water, and magnetic stirring was performed until the chitosan was completely dissolved. Then 0.1 g Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder was ultrasonicated for 20 min, heated and stirred at 45 °C for 4 h, washed with water 3 times, and then redispersed in 100 mL of deionized water, heated to 40 °C, and then 5 μL of 50% glutaraldehyde solution was added. The mixture was stirred for 4 h for cross-linking reaction, and then washed with deionized water and anhydrous ethanol for 5 times respectively, and then transferred to an oven at 80 °C for 10 h to obtain CS@LATP nanoparticles.
[0049] 2. Preparation of electrolyte:
[0050] CS@LATP nanoparticles were added to N,N-dimethylformamide (DMF) and ultrasonicated for 20 minutes, then PVDF-HFP and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were added, and heated at 50°C with magnetic stirring for 12 hours to obtain a casting solution; the casting solution was vacuum degassed and poured on a glass plate with a groove, and then placed on a heating plate at 40°C for 3 hours, and finally dried at 70°C for 12 hours to obtain an electrolyte membrane with a thickness of 100 μm; the electrolyte membrane was cut into discs with a diameter of 19 mm to obtain a chitosan-modified LATP benchmark solid electrolyte (PH-CS@LATP-2.5);
[0051] The mass fraction of CS@LATP nanoparticles in the casting solution described in step 2 is 2.5%;
[0052] The mass fraction of PVDF-HFP in the casting solution described in step 2 to N,N-dimethylformamide is 15%;
[0053] The mass ratio of LiTFSI to PVDF-HFP in the casting solution described in step 2 is 1:3.
[0054] Figure 1 The SEM and EDX element images of the CS@LATP nanoparticles prepared in step 1 of Example 1;
[0055] The microscopic morphology of the CS@LATP nanoparticles prepared in step 1 of Example 1 is as follows: Figure 1 As shown, the magnification of the scanning electron microscope image is 5k. From the EDX element image, it can be seen that the N element in chitosan is evenly distributed.
[0056] Figure 2 The SEM images of the plane and cross section of PH-LATP-Free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, where a, b and c are planes, and d, e and f are cross sections;
[0057] Figure 2 (a, b and c) show the surface scanning electron microscopy images of PH-LATP-Free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, respectively. The magnification is 1k. It can be seen that the surface of PH-LATP-Free electrolyte membrane is smooth and flat. From the cross-sectional view ( Figure 2 (d)) also shows no obvious holes. Compared with PH-CS@LATP-2.5, the surface of PH-LATP-2.5 electrolyte membrane is rougher. Figure 2 Obvious holes can be seen in (e), which is due to the huge difference in surface energy between LATP and polymer. Due to the introduction of chitosan intermediate layer between LATP and polymer substrate, LATP and PVDF-HFP polymer substrate are closely connected. Therefore, PH-CS@LATP-2.5 electrolyte membrane presents a dense morphology ( Figure 2 (f)). The close connection between the inorganic filler and the polymer is conducive to the uniform transmission of lithium ions, thereby suppressing lithium dendrites.
[0058] Figure 3 XRD patterns of PH-LATP-free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes;
[0059] Figure 3It can be seen that the polymer electrolyte before doping has a high intensity and sharp crystal peak near 2θ of 20°, which belongs to the polymer peak of PVDF-HFP (PDF#42-1650). After doping, it can be seen that the corresponding peak is generated at the position corresponding to the standard crystal card JCPDS#35-0754 of LiTi2(PO4)3, indicating that LATP and CS@LATP nanoparticles are doped into the electrolyte membrane.
[0060] Figure 4 a in the figure is the Arrhenius curve of PH-LATP-free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes. Figure 4 b is the lithium ion migration number of PH-CS@LATP-2.5 electrolyte membrane, Figure 4 c in the middle is the electrochemical stability window of PH-CS@LATP-2.5 electrolyte membrane;
[0061] Figure 4 (a) is the Arrhenius curve of the quasi-solid electrolyte before and after doping. The activation energies of PH-LATP-Free, PH-LATP-2.5 and PH-CS@LATP-2.5 electrolytes are 0.44, 0.39 and 0.33 eV, respectively, indicating that Li+ is more easily transferred in PH-CS@LATP-2.5 electrolyte. The lithium ion transfer number of PH-CS@LATP-2.5 electrolyte is about 0.28 ( Figure 4 (b) By doping CS@LATP nanoparticles, the ionic conductivity of the quasi-solid electrolyte is significantly enhanced, and the ionic conductivity before doping is 4.9×10 –5 Scm –1 After doping, the ionic conductivity increased to 2.6×10 –4 Scm –1 , indicating that the doping of well-dispersed CS@LATP nanoparticles significantly improved the electrochemical performance of the quasi-solid-state electrolyte; the electrochemical stability window of the quasi-solid-state electrolyte was tested by linear sweep voltammetry ( Figure 4 (c)), the oxidation potential of the doped electrolyte is as high as 5.07 V, which can meet the working requirements of lithium battery positive electrode materials.
[0062] Assembling a lithium symmetric cell:
[0063] In order to evaluate the practical applicability of the prepared electrolyte membrane in lithium metal batteries, a lithium symmetric battery with lithium metal as both positive and negative electrodes was assembled using CR2032 button cells. When assembling the lithium symmetric battery, the PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes were transferred to a glove box filled with argon gas, and 2μL of lithium electrolyte was dripped on both sides of the PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes to improve the interface contact between the electrode and the electrolyte; the lithium electrolyte was obtained by dissolving LiPF6 in a mixture of EC, DEC and EMC, wherein the volume ratio of EC, DEC and EMC in the mixture was 1:1:1; the concentration of LiPF6 was 1mol / L.
[0064] The limiting current density of the quasi-solid electrolyte was characterized by assembling lithium symmetric cells, e.g. Figure 5 As shown;
[0065] Figure 5 is the limiting current density of PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes;
[0066] from Figure 5 It can be seen that the limiting current density of the undoped quasi-solid electrolyte is 0.4 mA cm –2 After doping with CS@LATP nanoceramics, the limiting current density is increased to 1.0 mA cm –2 , the surface inhibition effect on lithium dendrites is enhanced.
[0067] Assembled lithium symmetric battery, at 0.05mAcm –2 The current density and 0.05 mAh cm –2 The life of the product was tested under the surface capacity of Figure 6 ); Figure 6 The lifespan of symmetric batteries assembled using PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, respectively;
[0068] from Figure 6 It can be seen that after about 125 hours of cycling, the overpotential of the symmetrical battery of the undoped quasi-solid electrolyte began to expand rapidly, indicating that the interface deteriorated and the impedance rose rapidly. After doping with 2.5% CS@LATP nanoceramics, the life of the quasi-solid electrolyte was significantly improved. The assembled symmetrical battery not only had a lower overpotential, but also could operate stably for more than 1800 hours.
[0069] Assembling quasi-solid-state batteries:
[0070] In order to evaluate the practical applicability of the prepared electrolyte membrane in lithium metal batteries, a full battery with a positive electrode of LiFePO4 and a negative electrode of lithium metal was assembled using CR2032 button cells. When assembling the full battery, the PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes were transferred to a glove box filled with argon gas, and 2μL of lithium battery electrolyte was dripped on both sides of the PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes to improve the interface contact between the electrode and the electrolyte; the lithium battery electrolyte was obtained by dissolving LiPF6 in a mixture of EC, DEC and EMC, wherein the volume ratio of EC, DEC and EMC in the mixture of EC, DEC and EMC was 1:1:1; the concentration of LiPF6 was 1mol / L.
[0071] Figure 7 Demonstrated the rate performance of a battery assembled from a LiFePO4 cathode, a quasi-solid electrolyte, and a lithium metal anode;
[0072] Figure 7 The rate performance curves of quasi-solid-state batteries assembled using PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes, respectively;
[0073] from Figure 7 It can be seen that the battery assembled with PH-LATP-2.5 quasi-solid electrolyte has a capacity of 158.1 mAhg at a rate of 0.1C. –1 The discharge capacity of the battery is 54.4 mAh g / cm2, but as the charge and discharge rate increases, the discharge capacity decreases. When the rate increases to 2C, the discharge capacity is only 54.4 mAh g / cm2. –1 After chitosan coating to improve the dispersibility of LATP, the battery assembled with PH-CS@LATP-2.5 quasi-solid electrolyte not only showed 161.9 mAhg at a rate of 0.1C, but also –1 The high discharge capacity is 114.6 mAh g even if the rate is increased to 2C. –1 The specific capacity of the modified quasi-solid electrolyte proves that it has excellent rate performance, can work at high current density and achieve fast charge and discharge.
[0074] Figure 8 Demonstrated the cycling performance of quasi-solid-state batteries at 0.5C rate;
[0075] Figure 8 The cycling performance curves of quasi-solid-state batteries assembled with PH-LATP-2.5 and PH-CS@LATP-2.5 electrolyte membranes at a rate of 0.5C are shown;
[0076] from Figure 8It can be seen that the initial discharge capacity of the battery assembled using PH-LATP-2.5 quasi-solid electrolyte is about 139.1 mAhg –1 After 700 cycles, it dropped to 79.9 mAh g –1 The capacity retention rate is 57.4%, while the performance of the battery assembled with PH-CS@LATP-2.5 quasi-solid electrolyte is significantly enhanced, with 141.6 mAh g at 0.5C. –1 The initial discharge capacity is 102.1 mAh g after 700 cycles. –1 The capacity retention rate is greater than 72.2%, indicating that after the doping modification of CS@LATP nanoparticles, the electrochemical performance of the quasi-solid electrolyte is effectively improved, and the assembled battery has excellent cycle performance and discharge capacity.
Claims
1. A method for preparing a chitosan-modified LATP-based solid electrolyte, characterized in that The preparation method is specifically completed according to the following steps:
1. Preparation of CS@LATP nanoparticles: Chitosan was added to a mixed solution of glacial acetic acid and deionized water, and magnetic stirring was performed until the chitosan was completely dissolved. Then Li 1.3 Al 0.3 Ti 1.7 (PO4)3 powder was ultrasonicated for a period of time, heated and stirred for a period of time, washed with water several times, and then redispersed in deionized water, heated to 35℃~45℃, and then added with 45%~55% glutaraldehyde solution by mass, stirred continuously for a period of time for cross-linking reaction, and then washed with deionized water and anhydrous ethanol several times in turn, and dried to obtain CS@LATP nanoparticles; The volume ratio of the chitosan mass described in step 1 to the mixed solution of glacial acetic acid and deionized water is 0.1 g: (95 mL to 10 mL); Li described in step 1 1.3 Al 0.3 Ti 1.7 The volume ratio of the mass of (PO4)3 powder to the mixed solution of glacial acetic acid and deionized water is 0.1g:(95mL~100mL); The ultrasonic time in step 1 is 20 min to 40 min; the heating and stirring temperature in step 1 is 40° C. to 50° C., and the heating and stirring time is 3 h to 5 h; 2. Preparation of electrolyte: The CS@LATP nanoparticles were added to N,N-dimethylformamide, ultrasonicated for a period of time, and then PVDF-HFP and LiTFSI were added, and heated and magnetically stirred for a period of time to obtain a casting solution; the casting solution was vacuum degassed and poured on a glass plate with a groove, and then placed on a heating plate to dry for a period of time, and finally dried at 70°C to 80°C for a period of time to obtain an electrolyte membrane; the electrolyte membrane was cut into discs to obtain a chitosan-modified LATP reference solid electrolyte; The mass fraction of CS@LATP nanoparticles in the casting solution described in step 2 is 0.5% to 7%; the mass fraction of PVDF-HFP in the casting solution described in step 2 is 15% of N,N-dimethylformamide; the mass ratio of LiTFSI to PVDF-HFP in the casting solution described in step 2 is 1:
3.
2. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that The volume ratio of glacial acetic acid to deionized water in the mixed solution of glacial acetic acid and deionized water described in step 1 is (2-5):(95-98).
3. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that The mass volume ratio of the chitosan described in step 1, the glutaraldehyde solution with a mass fraction of 45% to 55%, and the deionized water is 0.1 g: (4 μL to 6 μL): 100 mL.
4. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that The number of times of washing with water in step 1 is 3 to 5 times.
5. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that The cross-linking reaction time in step 1 is 3 h to 5 h; in step 1, deionized water and anhydrous ethanol are used for washing 3 to 5 times respectively.
6. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that The ultrasonic time described in step 2 is 20min to 30min; the temperature of the heating magnetic stirring described in step 2 is 45°C to 55°C, and the heating magnetic stirring time is 10h to 12h; the vacuum degassing time described in step 2 is 20min to 40min.
7. The method for preparing a chitosan-modified LATP reference solid electrolyte according to claim 1, characterized in that In step 2, the electrolyte membrane is placed on a heating plate at a temperature of 35°C to 45°C and dried for 2h to 4h, and finally dried at 70°C to 80°C for 10h to 12h; the thickness of the electrolyte membrane in step 2 is 100μm to 140μm; in step 2, the electrolyte membrane is cut into discs with a diameter of 16mm.
8. Application of a chitosan-modified LATP reference solid electrolyte prepared by the preparation method according to claim 1, characterized in that A chitosan-modified LATP-based solid electrolyte for application in lithium metal batteries.
9. The use of a chitosan-modified LATP reference solid electrolyte according to claim 8, characterized in that When a chitosan-modified LATP reference solid electrolyte is used in a lithium metal battery, it is transferred to a glove box filled with argon, and 2 μL of lithium battery electrolyte is dripped on both sides of the electrolyte to improve the interface contact between the electrode and the electrolyte; the lithium battery electrolyte is obtained by dissolving LiPF6 in a mixture of EC, DEC and EMC, wherein the volume ratio of EC, DEC and EMC in the mixture is 1:1:1; the concentration of LiPF6 is 1 mol / L.
Citation Information
Patent Citations
Application of chitosan polymer in solid electrolyte membrane
CN106785028A
Inorganic solid electrolyte-cellulose composite diaphragm and preparation method thereof
CN108470875A
In-situ self-forming preparation method for composite polymer solid electrolyte membrane
CN108484836A
Preparation method for NASICON type solid electrolyte
CN109742449A