Anti-skid and wear-resistant EVA composite shoe material and preparation method thereof
By adding modified talc powder and composite nano silica to EVA composite shoe materials and using specific process treatment, the problems of poor high and low temperature resistance and insufficient anti-slip properties in shoe materials are solved, which significantly improves the The wear resistance and slip resistance of the shoe material extend the service life.
Patent Information
- Application Number
- CN202410192048.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-02-21
AI Technical Summary
The existing EVA foaming materials have problems in shoe materials such as poor high and low temperature resistance, poor rebound, poor wear resistance and slip resistance, which affects the service life of shoe materials.
EVA, modified talc powder, polyamide elastomer, composite nanosilica, compatibilizer, foaming agent and zinc stearate for intensive refining, molding and electronic irradiation treatment. By adjusting process parameters and components, the preparation is prepared. Unslip and wear-resistant EVA composite shoe material.
It improves the elasticity, wear resistance, slip resistance and water resistance of the shoe material, enhances the mechanical strength and impact resistance, and extends the service life.
Smart Images

Figure BDA0004708288600000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of shoe materials, in particular to a non-slip and wear-resistant EVA composite shoe material and a preparation method thereof. Background Art
[0002] As people's consumption level improves, the requirements for shoe materials are also constantly increasing. They are not only satisfied with the practicality of shoe materials, but also have higher requirements for shoe materials' lightness, anti-slip, wear resistance and other functions.
[0003] The sole materials of shoes on the market generally require lightweight characteristics. Ethylene vinyl acetate copolymer (EVA) foam material is a porous material composed of gas and solid phases. It has good sound insulation, noise reduction, cushioning and shock absorption, easy processing and other properties. It is one of the raw materials for preparing shoes on the current market. However, EVA foam material has defects such as poor high and low temperature resistance, poor resilience, poor wear resistance and anti-slip properties, which affect the service life of the shoe material. Summary of the invention
[0004] The object of the present invention is to provide a non-slip and wear-resistant EVA composite shoe material and a preparation method thereof, so as to solve the problems in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a non-slip and wear-resistant EVA composite shoe material comprises the following steps:
[0007] S1: Put EVA, modified talc, polyamide elastomer, composite nano-silica, compatibilizer, foaming agent and zinc stearate into an internal mixer and mix them to obtain a blended material;
[0008] S2: The blended material is placed in a flat vulcanizer for molding, electron irradiation treatment, and foaming molding to obtain an anti-skid and wear-resistant EVA composite shoe material.
[0009] Furthermore, the working conditions of the molding are: working temperature is 120° C., time is 2 min, and molding pressure is 10 MPa.
[0010] Furthermore, the working conditions of the electron irradiation treatment are: through an electron accelerator, the irradiation dose is 68 kGy, and the irradiation time is 5 min.
[0011] Furthermore, the working conditions of the foaming molding are: working temperature is 240° C., and the foaming time is 2 min.
[0012] Furthermore, the foaming agent is azodicarbonamide, and the compatibilizer is ethylene-vinyl acetate grafted maleic anhydride.
[0013] Furthermore, the composition of the blended material is, by mass fraction, 72-82 parts of EVA, 5-7 parts of modified talc, 18-22 parts of polyamide elastomer, 1-3 parts of composite nano-silicon dioxide, 1-2 parts of compatibilizer, 8-12 parts of foaming agent, and 1-3 parts of zinc stearate.
[0014] Further, the preparation of composite nano-silicon dioxide comprises the following steps:
[0015] 1) Under an argon atmosphere, chloroplatinic acid, toluene, allyl glycidyl ether and dodecene are mixed, the temperature is raised to 78-80° C., hydrogen-containing polysiloxane is added, the temperature is kept for 6-7 hours, and the epoxy polysiloxane is obtained by rotary evaporation;
[0016] 2) mixing nano-silica and toluene, keeping the mixture at 75-80° C. for 8-10 min, adding dodecyltrimethoxysilane, keeping the mixture for 8-9 h, adding epoxy polysiloxane, keeping the mixture for 7-8 h, centrifuging, washing, centrifuging, drying, and grinding to obtain modified nano-silica;
[0017] 3) In an argon atmosphere, the polyamino branched polyamide, methanol and modified nano-silica are mixed, kept at 18-25° C. for 3-4 days, rotary evaporated, transferred into distilled water, dialyzed with distilled water for 12 hours, and freeze-dried to obtain composite nano-silica.
[0018] Further, the preparation of modified talcum powder comprises the following steps:
[0019] (1) mixing talc powder and sodium hydroxide solution, keeping the mixture at 88-90° C. for 5-6 hours, cooling, washing, centrifuging, and drying to obtain hydroxylated talc powder;
[0020] (2) mixing hydroxylated talc, ethanol and distilled water, adjusting the pH to 6.2-6.4, adding 3-(isobutyleneoxy)propyltrimethoxysilane, keeping in a water bath at 83-87° C. for 5-6 hours, cooling, centrifuging, washing with anhydrous ethanol for 3-5 times, and drying to obtain allylated talc;
[0021] (3) The polyamino branched polyamide, methanol and allyl talc are mixed, kept at 18-25° C. for 46-48 hours, dialyzed with ethanol for 12 hours, and rotary evaporated to obtain modified talc.
[0022] Further, the preparation of the polyamino branched polyamide comprises the following steps:
[0023] A. In an ice water bath, concentrated hydrochloric acid and furanamine are mixed, levulinic acid is added, the temperature is raised to 48-50°C and kept for 23-24 hours, washed, centrifuged, dried, added to distilled water, sodium hydroxide is added, washed three times with dichloromethane, separated, rotary evaporated, filtered, concentrated hydrochloric acid is added to precipitate solids, washed, centrifuged, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride;
[0024] B. Under argon protection, 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride, anhydrous methanol and p-toluenesulfonic acid monohydrate were mixed, refluxed for 6-7h, rotary evaporated, washed with isopropanol, filtered and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride; sodium hydroxide and distilled water were mixed, and a mixture of 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride, distilled water and chloroform was added, the mixture was allowed to stand for separation, and rotary evaporated to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester;
[0025] C. In an argon atmosphere, the temperature of methyl 4,4'-bis(5-amino-2-furyl)pentanoate was raised to 70-75°C and kept for 46-48 hours, then raised to 98-100°C and kept for 3 hours, methanol was added, and then transferred to a sodium chloride solution for precipitation, filtered, and dried to obtain a polyamino branched polyamide.
[0026] Beneficial effects of the present invention:
[0027] The invention provides a non-slip and wear-resistant EVA composite shoe material and a preparation method thereof. By adjusting the composition and process of the shoe material, the prepared composite shoe material has good elasticity, high wear resistance, non-slip property and waterproof property.
[0028] In view of the shortcomings of EVA in shoe materials, the present invention selects polyamide elastomer and EVA with excellent wear resistance, low and high temperature resistance, antistatic property and resilience as base materials, selects azodicarbonamide as a foaming agent, ethylene-vinyl acetate grafted maleic anhydride as a compatibilizer, adopts radiation cross-linking composite foaming, and controls its process parameters to prepare a softer and more elastic base material, thereby greatly improving the mechanical strength of the shoe material.
[0029] The invention improves the wear resistance, skid resistance and water resistance of the shoe material by introducing nano silicon dioxide and talcum powder. In order to improve the uniformity of the dispersion of nano silicon dioxide and talcum powder in the base material, the nano silicon dioxide and talcum powder are modified in sequence. The invention uses allyl glycidyl ether, dodecene and hydrogen-containing polysiloxane to synthesize epoxy polysiloxane, and then modifies the nano silicon dioxide with dodecyl trimethoxy silane to prepare epoxidized hydrophobic nano silicon dioxide powder. Then, the epoxy-amino reaction is used to synthesize epoxy polysiloxane. The composite silica was obtained by grafting polyamino branched polyamide, which was added to the base material as a filler to greatly improve the wear resistance and waterproofness of the shoe material. The polyamino branched polyamide was synthesized from renewable levulinic acid and furanamine to obtain 4,4'-bis(5-amino-2-furanyl) methyl pentanoate, which was prepared by self-condensation under melt conditions. The introduction of polyamino branched polyamide effectively improved the compatibility between nano-silica and the base polyamide, achieving permanent wear resistance and waterproof performance.
[0030] The present invention sequentially hydroxylates and allylates the surface of talc powder, and then utilizes the reaction between amino groups and double bonds to graft polyamino branched polyamide on the surface of talc powder, thereby improving the uniformity of talc powder dispersion in the base material and improving the impact resistance and waterproofness of the shoe material. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.
[0033] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0034] Embodiment 1: A method for preparing a non-slip and wear-resistant EVA composite shoe material, comprising the following steps:
[0035] S1: Put EVA, modified talc, polyamide elastomer, composite nano-silica, compatibilizer, foaming agent and zinc stearate into an internal mixer and mix them to obtain a blended material;
[0036] The composition of the blended material is as follows: 72 parts of EVA, 5 parts of modified talc, 18 parts of polyamide elastomer, 1 part of composite nano-silicon dioxide, 1 part of compatibilizer, 8 parts of foaming agent, and 1 part of zinc stearate by mass fraction;
[0037] The foaming agent is azodicarbonamide; the compatibilizer is ethylene-vinyl acetate grafted maleic anhydride;
[0038] The preparation of composite nano-silicon dioxide includes the following steps:
[0039] 1) Under an argon atmosphere, 1.8 g of chloroplatinic acid, 58 mL of toluene, 0.225 mol of allyl glycidyl ether, and 0.075 mol of dodecene were mixed, the temperature was raised to 78° C., 0.25 mol of hydrogen-containing polysiloxane was added, the temperature was kept for 6 h, and the epoxy polysiloxane was obtained by rotary evaporation;
[0040] 2) 0.5 g of nano-silica and 20 mL of toluene were mixed, kept warm at 75° C. for 10 min, 0.2 mL of dodecyltrimethoxysilane was added, and the mixture was kept warm for 8 h, 0.1 mL of epoxypolysiloxane was added, and the mixture was kept warm for 7 h, centrifuged, washed, centrifuged, dried, and ground to obtain modified nano-silica;
[0041] 3) Under an argon atmosphere, 1.2 g of polyamino branched polyamide, 10 mL of methanol, and 0.62 g of modified nano-silica were mixed, kept at 18°C for 4 days, rotary evaporated, transferred into 200 mL of distilled water, dialyzed with distilled water for 12 hours, and freeze-dried to obtain composite nano-silica;
[0042] The preparation of modified talcum powder comprises the following steps:
[0043] (1) 5 g of talc and 50 mL of 30% sodium hydroxide solution were mixed, kept at 88° C. for 6 h, cooled, washed, centrifuged, and dried to obtain hydroxylated talc;
[0044] (2) 5 g of hydroxylated talc, 33 mL of ethanol, and 5 mL of distilled water were mixed, the pH was adjusted to 6.2, 1 g of 3-(isobutyleneoxy)propyltrimethoxysilane was added, and the mixture was kept in a water bath at 83° C. for 6 h, cooled, centrifuged, washed three times with anhydrous ethanol, and dried to obtain allylated talc;
[0045] (3) 1 g of polyamino branched polyamide, 10 mL of methanol, and 0.44 g of allylated talc were mixed, kept at 18° C. for 48 h, dialyzed with ethanol for 12 h, and rotary evaporated to obtain modified talc;
[0046] The preparation of polyamino branched polyamide comprises the following steps:
[0047] A. In an ice water bath, 10 mL of concentrated hydrochloric acid and 3.64 g of furanylamine were mixed, 2.17 g of levulinic acid was added, the temperature was raised to 48°C and kept for 24 h, washed, centrifuged, dried, added to 100 mL of distilled water, 200 mL of sodium hydroxide was added, washed three times with dichloromethane, separated, rotary evaporated, filtered, concentrated hydrochloric acid was added to precipitate solids, washed, centrifuged, and dried to obtain 4,4'-bis(5-amino-2-furanyl)pentanoic acid hydrochloride;
[0048] B. Under argon protection, 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride, 200 mL of anhydrous methanol, and 0.12 g of p-toluenesulfonic acid monohydrate were mixed, refluxed for 6 h, rotary evaporated, washed with isopropanol, filtered, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride; 1.1 g of sodium hydroxide and 5 mL of distilled water were mixed, and a mixture of 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride, 20 mL of distilled water, and 100 mL of chloroform was added, the mixture was allowed to stand for separation, and rotary evaporated to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester;
[0049] C. In an argon atmosphere, 3 g of 4,4'-bis(5-amino-2-furyl) methyl pentanoate was heated to 70°C and kept for 48 h, then heated to 98°C and kept for 3 h, 10 mL of methanol was added, and then transferred to 200 mL of sodium chloride solution for precipitation, filtered, and dried to obtain a polyamino branched polyamide;
[0050] S2: placing the blended material in a flat vulcanizer for molding, electron irradiation treatment, and foaming molding to obtain an anti-skid and wear-resistant EVA composite shoe material;
[0051] The working conditions of the molding are: working temperature is 120°C, time is 2min, and molding pressure is 10MPa;
[0052] The working conditions of electron irradiation treatment are: irradiation dose of 68 kGy and irradiation time of 5 min through electron accelerator;
[0053] The working conditions of foaming molding are: in a vertical foaming furnace, the working temperature is 240°C and the foaming time is 2 minutes.
[0054] Embodiment 2: A method for preparing a non-slip and wear-resistant EVA composite shoe material, comprising the following steps:
[0055] S1: Put EVA, modified talc, polyamide elastomer, composite nano-silica, compatibilizer, foaming agent and zinc stearate into an internal mixer and mix them to obtain a blended material;
[0056] The composition of the blended material is as follows: 77 parts of EVA, 6 parts of modified talc, 19 parts of polyamide elastomer, 2 parts of composite nano-silicon dioxide, 1.5 parts of compatibilizer, 10 parts of foaming agent, and 2 parts of zinc stearate, by mass fraction.
[0057] The foaming agent is azodicarbonamide; the compatibilizer is ethylene-vinyl acetate grafted maleic anhydride;
[0058] The preparation of composite nano-silicon dioxide includes the following steps:
[0059] 1) Under an argon atmosphere, 1.8 g of chloroplatinic acid, 58 mL of toluene, 0.225 mol of allyl glycidyl ether, and 0.075 mol of dodecene were mixed, the temperature was raised to 79° C., 0.25 mol of hydrogen-containing polysiloxane was added, the temperature was kept for 6.5 h, and the epoxy polysiloxane was obtained by rotary evaporation;
[0060] 2) 0.5 g of nano-silica and 20 mL of toluene were mixed, kept warm at 78° C. for 9 min, 0.2 mL of dodecyltrimethoxysilane was added, and the mixture was kept warm for 8.5 h, 0.1 mL of epoxypolysiloxane was added, and the mixture was kept warm for 7.5 h, centrifuged, washed, centrifuged, dried, and ground to obtain modified nano-silica;
[0061] 3) Under an argon atmosphere, 1.2 g of polyamino branched polyamide, 10 mL of methanol, and 0.62 g of modified nano-silica were mixed, kept at 20° C. for 3.5 days, rotary evaporated, transferred to 200 mL of distilled water, dialyzed with distilled water for 12 hours, and freeze-dried to obtain composite nano-silica;
[0062] The preparation of modified talcum powder comprises the following steps:
[0063] (1) 5 g of talc and 50 mL of 30% sodium hydroxide solution were mixed, kept at 89° C. for 5.5 h, cooled, washed, centrifuged, and dried to obtain hydroxylated talc;
[0064] (2) 5 g of hydroxylated talc, 33 mL of ethanol, and 5 mL of distilled water were mixed, the pH was adjusted to 6.3, 1 g of 3-(isobutyleneoxy)propyltrimethoxysilane was added, and the mixture was kept in a water bath at 85° C. for 5.5 h, cooled, centrifuged, washed with anhydrous ethanol 4 times, and dried to obtain allylated talc;
[0065] (3) 1 g of polyamino branched polyamide, 10 mL of methanol, and 0.44 g of allylated talc were mixed, kept at 20° C. for 47 h, dialyzed with ethanol for 12 h, and rotary evaporated to obtain modified talc;
[0066] The preparation of the polyamino branched polyamide comprises the following steps: A. In an ice water bath, 10 mL of concentrated hydrochloric acid and 3.64 g of furanylamine are mixed, 2.17 g of levulinic acid is added, the temperature is raised to 49° C. and kept for 23.5 h, washed, centrifuged, dried, added to 100 mL of distilled water, 200 mL of sodium hydroxide is added, washed three times with dichloromethane, separated, rotary evaporated, filtered, concentrated hydrochloric acid is added to precipitate solids, washed, centrifuged, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride;
[0067] B. Under argon protection, 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride, 200 mL of anhydrous methanol, and 0.12 g of p-toluenesulfonic acid monohydrate were mixed, refluxed for 6.5 h, rotary evaporated, washed with isopropanol, filtered, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride; 1.1 g of sodium hydroxide and 5 mL of distilled water were mixed, and a mixture of 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride, 20 mL of distilled water, and 100 mL of chloroform was added, the mixture was allowed to stand for separation, and rotary evaporated to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester;
[0068] C. In an argon atmosphere, 3 g of 4,4'-bis(5-amino-2-furyl) methyl pentanoate was heated to 73°C and kept for 47 h, then heated to 99°C and kept for 3 h, 10 mL of methanol was added, and then transferred to 200 mL of sodium chloride solution for precipitation, filtered, and dried to obtain a polyamino branched polyamide;
[0069] S2: placing the blended material in a flat vulcanizer for molding, electron irradiation treatment, and foaming molding to obtain an anti-skid and wear-resistant EVA composite shoe material;
[0070] The working conditions of the molding are: working temperature is 120°C, time is 2min, and molding pressure is 10MPa;
[0071] The working conditions of electron irradiation treatment are: irradiation dose of 68 kGy and irradiation time of 5 min through electron accelerator;
[0072] The working conditions of foaming molding are: in a vertical foaming furnace, the working temperature is 240°C and the foaming time is 2 minutes.
[0073] Embodiment 3: A method for preparing a non-slip and wear-resistant EVA composite shoe material, comprising the following steps:
[0074] S1: Put EVA, modified talc, polyamide elastomer, composite nano-silica, compatibilizer, foaming agent and zinc stearate into an internal mixer and mix them to obtain a blended material;
[0075] The composition of the blended material is as follows: 82 parts of EVA, 7 parts of modified talc, 22 parts of polyamide elastomer, 3 parts of composite nano-silicon dioxide, 2 parts of compatibilizer, 12 parts of foaming agent, and 3 parts of zinc stearate, by mass fraction.
[0076] The foaming agent is azodicarbonamide; the compatibilizer is ethylene-vinyl acetate grafted maleic anhydride;
[0077] The preparation of composite nano-silicon dioxide includes the following steps:
[0078] 1) Under an argon atmosphere, 1.8 g of chloroplatinic acid, 58 mL of toluene, 0.225 mol of allyl glycidyl ether, and 0.075 mol of dodecene were mixed, the temperature was raised to 80° C., 0.25 mol of hydrogen-containing polysiloxane was added, the temperature was kept for 7 h, and the epoxy polysiloxane was obtained by rotary evaporation;
[0079] 2) 0.5 g of nano-silica and 20 mL of toluene were mixed, kept warm at 80° C. for 8 min, 0.2 mL of dodecyltrimethoxysilane was added, and the mixture was kept warm for 9 h, 0.1 mL of epoxypolysiloxane was added, and the mixture was kept warm for 8 h, centrifuged, washed, centrifuged, dried, and ground to obtain modified nano-silica;
[0080] 3) Under an argon atmosphere, 1.2 g of polyamino branched polyamide, 10 mL of methanol, and 0.62 g of modified nano-silica were mixed, kept at 25°C for 3 days, rotary evaporated, transferred into 200 mL of distilled water, dialyzed with distilled water for 12 hours, and freeze-dried to obtain composite nano-silica;
[0081] The preparation of modified talcum powder comprises the following steps:
[0082] (1) 5 g of talc and 50 mL of 30% sodium hydroxide solution were mixed, kept at 90° C. for 5 h, cooled, washed, centrifuged, and dried to obtain hydroxylated talc;
[0083] (2) 5 g of hydroxylated talc, 33 mL of ethanol, and 5 mL of distilled water were mixed, the pH was adjusted to 6.4, 1 g of 3-(isobutyleneoxy)propyltrimethoxysilane was added, and the mixture was kept in a water bath at 87° C. for 5 h, cooled, centrifuged, washed with anhydrous ethanol 5 times, and dried to obtain allylated talc;
[0084] (3) 1 g of polyamino branched polyamide, 10 mL of methanol, and 0.44 g of allylated talc were mixed, kept at 25° C. for 46 h, dialyzed with ethanol for 12 h, and rotary evaporated to obtain modified talc;
[0085] The preparation of the multi-amino branched polyamide comprises the following steps: A. In an ice water bath, 10 mL of concentrated hydrochloric acid and 3.64 g of furanylamine are mixed, 2.17 g of levulinic acid is added, the temperature is raised to 50° C. and kept for 23 hours, washed, centrifuged, dried, added to 100 mL of distilled water, 200 mL of sodium hydroxide is added, washed three times with dichloromethane, separated, rotary evaporated, filtered, concentrated hydrochloric acid is added to precipitate solids, washed, centrifuged, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride;
[0086] B. Under argon protection, 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride, 200 mL of anhydrous methanol, and 0.12 g of p-toluenesulfonic acid monohydrate were mixed, refluxed for 7 h, rotary evaporated, washed with isopropanol, filtered, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride; 1.1 g of sodium hydroxide and 5 mL of distilled water were mixed, and a mixture of 5 g of 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride, 20 mL of distilled water, and 100 mL of chloroform was added, the mixture was allowed to stand for separation, and rotary evaporated to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester;
[0087] C. In an argon atmosphere, 3 g of 4,4'-bis(5-amino-2-furyl) methyl pentanoate was heated to 75°C and kept for 46 h, then heated to 100°C and kept for 3 h, 10 mL of methanol was added, and then transferred to 200 mL of sodium chloride solution for precipitation, filtered, and dried to obtain a polyamino branched polyamide;
[0088] S2: placing the blended material in a flat vulcanizer for molding, electron irradiation treatment, and foaming molding to obtain an anti-skid and wear-resistant EVA composite shoe material;
[0089] The working conditions of the molding are: working temperature is 120°C, time is 2min, and molding pressure is 10MPa;
[0090] The working conditions of electron irradiation treatment are: irradiation dose of 68 kGy and irradiation time of 5 min through electron accelerator;
[0091] The working conditions of foaming molding are: in a vertical foaming furnace, the working temperature is 240°C and the foaming time is 2 minutes.
[0092] Comparative Example 1: Example 3 was used as a control group, in which no polyamino branched polyamide was prepared, and other processes were normal.
[0093] Comparative Example 2: Taking Example 3 as the control group, talcum powder was used to replace the modified talcum powder, and the other processes were normal.
[0094] Comparative Example 3: Taking Example 3 as the control group, nano silicon dioxide was used to replace the composite nano silicon dioxide, and the other processes were normal.
[0095] The sources of raw materials used in the above examples and comparative examples are:
[0096] Hydrogenated polysiloxane 63148-57-2: Hubei Shixing Chemical Co., Ltd.; polyamide elastomer L1640: Dongguan Suguang Plastic Raw Materials Co., Ltd.; ethylene-vinyl acetate grafted maleic anhydride; EVAP301631, zinc stearate Z432906, azodicarbonamide A302276, chloroplatinic acid C139933, allyl glycidyl ether A106314, dodecene D106548, nano-silica S10 4596, dodecyltrimethoxysilane D155296, talc T109494, 3-(isobutyleneoxy)propyltrimethoxysilane S111153, furanamine F482060, levulinic acid L104281, p-toluenesulfonic acid monohydrate T104290: Aladdin reagent; isopropanol, toluene, methanol, sodium hydroxide, dichloromethane, concentrated hydrochloric acid, ethanol, sodium chloride, analytical grade: Sinopharm Chemical Reagent Co., Ltd.
[0097] Performance test: The shoe materials prepared in the embodiments and comparative examples were tested, and the test results are shown in Table 1;
[0098] Abrasion performance test: Tested with reference to GB / T9867-2008; Rebound rate: Tested with reference to GB / T10652-2001, the sample size is 120mm×120mm×60mm, record the maximum rebound height, and obtain 3 valid rebound values within 1min, and take the average value of 3 groups; Hydrophobicity: Characterized by water contact angle, tested with 4μL distilled water droplet; The specific results are shown in Table 1;
[0099] Table 1
[0100]
[0101] The invention provides a non-slip and wear-resistant EVA composite shoe material and a preparation method thereof. By adjusting the components of the shoe material, the prepared composite shoe material has good elasticity, high wear resistance and waterproofness.
[0102] By comparing Example 3 with Comparative Example 1, it can be seen that the introduction of polyamino branched polyamide effectively improves the compatibility between nano-silicon dioxide, talcum powder and base polyamide, achieving permanent wear resistance and waterproof performance.
[0103] By comparing Example 3 with Comparative Example 2, it can be seen that epoxy polysiloxane is synthesized with allyl glycidyl ether, dodecene, and hydrogen-containing polysiloxane, and then nano-silica is modified with dodecyltrimethoxysilane to prepare epoxidized super-hydrophobic nano-silica powder, and then polyamino branched polyamide is grafted by epoxy-amino reaction to obtain composite silica, which is added to the base material as a filler to greatly improve the wear resistance and waterproofness of the shoe material.
[0104] By comparing Example 3 with Comparative Example 3, it can be seen that the surface of talc powder is hydroxylated and allylated in sequence, and then the amino group reacts with the double bond to graft the polyamino branched polyamide on the surface of talc powder, thereby improving the uniformity of dispersion of talc powder and base material and improving the impact resistance of the shoe material.
[0105] The above descriptions are only embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a non-slip and wear-resistant EVA composite shoe material, characterized in that: The following steps are involved: S1: Put EVA, modified talc, polyamide elastomer, composite nano-silica, compatibilizer, foaming agent and zinc stearate into an internal mixer and mix them to obtain a blended material; S2: placing the blended material in a flat vulcanizer for molding, electron irradiation treatment, and foaming molding to obtain an anti-skid and wear-resistant EVA composite shoe material; The preparation of composite nano-silicon dioxide includes the following steps: 1) Under an argon atmosphere, chloroplatinic acid, toluene, allyl glycidyl ether and dodecene are mixed, the temperature is raised to 78-80° C., hydrogen-containing polysiloxane is added, the temperature is kept for 6-7 hours, and the epoxy polysiloxane is obtained by rotary evaporation; 2) mixing nano-silica and toluene, keeping the mixture at 75-80° C. for 8-10 min, adding dodecyltrimethoxysilane, keeping the mixture for 8-9 h, adding epoxy polysiloxane, keeping the mixture for 7-8 h, centrifuging, washing, centrifuging, drying, and grinding to obtain modified nano-silica; 3) In an argon atmosphere, the polyamino branched polyamide, methanol and modified nano-silica are mixed, kept at 18-25° C. for 3-4 days, rotary evaporated, transferred to distilled water, dialyzed with distilled water for 12 hours, and freeze-dried to obtain composite nano-silica; The preparation of modified talcum powder comprises the following steps: (1) mixing talc powder and sodium hydroxide solution, keeping the mixture at 88-90° C. for 5-6 hours, cooling, washing, centrifuging, and drying to obtain hydroxylated talc powder; (2) mixing hydroxylated talc, ethanol and distilled water, adjusting the pH to 6.2-6.4, adding 3-(isobutyleneoxy)propyltrimethoxysilane, keeping in a water bath at 83-87° C. for 5-6 hours, cooling, centrifuging, washing with anhydrous ethanol for 3-5 times, and drying to obtain allylated talc; (3) mixing the polyamino branched polyamide, methanol and allylated talc, keeping the mixture at 18-25° C. for 46-48 hours, dialyzing with ethanol for 12 hours, and rotary evaporating to obtain modified talc; The preparation of polyamino branched polyamide comprises the following steps: A. In an ice water bath, concentrated hydrochloric acid and furanamine are mixed, levulinic acid is added, the temperature is raised to 48-50°C and kept for 23-24 hours, washed, centrifuged, dried, added to distilled water, sodium hydroxide is added, washed three times with dichloromethane, separated, rotary evaporated, filtered, concentrated hydrochloric acid is added to precipitate solids, washed, centrifuged, and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride; B. Under argon protection, 4,4'-bis(5-amino-2-furanyl)valeric acid hydrochloride, anhydrous methanol and p-toluenesulfonic acid monohydrate were mixed, refluxed for 6-7h, rotary evaporated, washed with isopropanol, filtered and dried to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride; sodium hydroxide and distilled water were mixed, and a mixture of 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester hydrochloride, distilled water and chloroform was added, the mixture was allowed to stand for separation, and rotary evaporated to obtain 4,4'-bis(5-amino-2-furanyl)valeric acid methyl ester; C. In an argon atmosphere, the temperature of methyl 4,4'-bis(5-amino-2-furyl)pentanoate was raised to 70-75°C and kept for 46-48 hours, then raised to 98-100°C and kept for 3 hours, methanol was added, and then transferred to a sodium chloride solution for precipitation, filtered, and dried to obtain a polyamino branched polyamide.
2. The method for preparing a non-slip and wear-resistant EVA composite shoe material according to claim 1, characterized in that: The working conditions of the molding are: working temperature is 120°C, time is 2min, and molding pressure is 10MPa.
3. The method for preparing a non-slip and wear-resistant EVA composite shoe material according to claim 1, characterized in that: The working conditions of electron irradiation treatment are: through electron accelerator, irradiation dose is 68kGy, irradiation time is 5min.
4. The method for preparing a non-slip and wear-resistant EVA composite shoe material according to claim 1, characterized in that: The working conditions of foaming molding are: working temperature is 240℃ and foaming time is 2min.
5. The method for preparing a non-slip and wear-resistant EVA composite shoe material according to claim 1, characterized in that: The foaming agent is azodicarbonamide, and the compatibilizer is ethylene-vinyl acetate grafted maleic anhydride.
6. The method for preparing a non-slip and wear-resistant EVA composite shoe material according to claim 1, characterized in that: The blended material comprises, by weight, 72-82 parts of EVA, 5-7 parts of modified talc, 18-22 parts of polyamide elastomer, 1-3 parts of composite nano-silicon dioxide, 1-2 parts of compatibilizer, 8-12 parts of foaming agent and 1-3 parts of zinc stearate.
7. A non-slip and wear-resistant EVA composite shoe material, characterized in that: Prepared by the method according to any one of claims 1 to 6.