ReBCO protective layer processing method

Through the combination of physical vapor deposition and electroplating, the problems of island-like aggregation and hole defects during silver plating and copper plating of high-temperature superconducting strips are solved, forming a complete copper layer covering structure, improving bending performance and corrosion resistance , suitable for high-field magnet applications.

CN118127463BActive Publication Date: 2024-11-19SHANGHAI SUPERCONDUCTOR TECH CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410255785.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-11-19
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

In the prior art, high-temperature superconducting strips have island aggregation, hole defects and adhesion problems during silver plating and copper plating, resulting in incomplete cover of superconducting layer, easy to be corroded, and insufficient thickness of copper plating layer leads to bending. Poor performance and cannot meet the requirements of high-field magnets.

Method used

The protective layer is plating by physical vapor deposition method, the coating thickness is less than or equal to 2um. Combined with electroplating of copper, pre-copper plating, bright copper and sand-surface copper treatment, a complete copper layer covering structure is formed to avoid acid corrosion and internal corrosion. Excessive stress.

Benefits of technology

It achieves good bending performance of superconducting strips, avoids layering and hole corrosion, ensures the integrity and strength of the copper layer, and is suitable for high-field magnet applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127463B_ABST
    Figure CN118127463B_ABST
Patent Text Reader

Abstract

The present invention provides a ReBCO protective layer processing method, comprising the following steps: step 1: physically coating a superconducting tape by physical vapor deposition; step 2: chemically copper-plating the physically coated superconducting tape by electroplating copper. The present invention first performs physical coating and then chemical copper plating, thereby preventing the superconducting layer from being damaged during subsequent processing and use due to defects on the surface of the silver tape, and also solves the defects of excessive internal stress of the film layer and easy delamination of the tape when relying solely on physical vapor deposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ReBCO superconducting tape post-processing technology, and in particular to a ReBCO protective layer processing method. Background Art

[0002] At present, the practical superconducting materials discovered internationally mainly include low-temperature superconducting wires, bismuth-based high-temperature superconducting tapes, rare earth barium copper oxide coated conductors, MgB2 wires and tapes, and new iron-based superconducting wires and tapes. Among them, low-temperature superconductors represented by Nb-Ti and Nb3Sn have been commercialized, and their preparation processes and performance development have been fully mature and widely used. MgB2 superconducting materials will have a place in the application of MRI superconducting magnets in the range of 15-20K and 1-2T due to their relatively simple processing process and low raw material costs. Iron-based superconducting wires and tapes are in a rapid development stage of research and development. Its advantages are large current under strong magnetic fields and small anisotropy, and it is expected to become the main practical superconducting material for ultra-high field magnet applications in the temperature range of 4.2-30K. Oxide high-temperature superconducting materials (including first and second generations) will be the protagonists of strong electric applications in the liquid nitrogen temperature range, and their application prospects are broad. In particular, the second-generation high-temperature superconducting tapes represented by rare earth barium copper oxide coated conductors are on the eve of industrialization and are rapidly developing towards stabilization and scale. Their excellent external field current carrying capacity and potential cost advantages make them extremely irreplaceable and they are recognized as true superconducting materials for applications in strong electric and magnetic fields at liquid nitrogen temperature ranges.

[0003] The second generation of high temperature superconducting tapes (also called coated conductors) made of rare earth barium copper oxides have better performance under magnetic fields. The irreversible field at 77K reaches 7T, which is an order of magnitude higher than Bi-2223. It is a true superconducting material for strong electrical applications in the liquid nitrogen temperature range. The main obstacle to obtaining high-performance second generation high temperature superconducting tapes (such as YBCO) is the weak connection problem. The grain boundary angle between adjacent YBCO grains is the key to determining whether the superconductor can carry unimpeded large currents. In addition, since the current transmission of YBCO is mainly within its ab plane, in order to obtain high-performance second generation high temperature superconducting tapes, it is necessary to first prepare a crystallographically neatly arranged YBCO layer on a flexible metal substrate. At present, there are several industrial technologies that can deposit thin films on a large scale, such as PLD, MOCVD, MOD, evaporation technology, etc. These technologies may become the choice for large-scale preparation of second generation high temperature superconducting tapes.

[0004] High-temperature superconducting coated conductors are mainly composed of a metal base tape, a buffer layer, a RE123 superconducting layer, a protective layer, etc. The metal base tape is generally Ni or a Ni alloy (such as Hastelloy) with a very high flatness, or even stainless steel, with a thickness of 50 to 100 μm. The base tape must have a buffer layer of different types of oxides and thicknesses, and the top buffer layer grains must have a biaxial texture feature, which is constructed by epitaxially growing the texture of the metal base tape or by ion beam assisted deposition. Subsequently, a 0.6 to 3 μm RE123 superconducting layer is epitaxially grown, and then covered with a few microns of silver as a protective layer, and finally a stabilization layer is plated or armored.

[0005] The protective layer is mainly used to protect the superconducting film layer. Generally, a 0.5-5μm silver layer is plated on the front and back surfaces of the superconducting tape by magnetron sputtering or evaporation. In order to pursue lower material costs, the silver layer on the superconducting surface is usually set at 1-2μm, and the silver layer on the non-superconducting surface is usually set at 0.5-1μm. The superconducting tape with a silver layer on the surface needs to go through an annealing process to make it have superconducting properties. Then, according to the requirements of the specific application for the width of the tape, the 10-12mm tape is cut into 2-8mm. Finally, copper plating or subsequent packaging reinforcement treatment is carried out. The copper plating thickness of the subsequent packaged tape can be 1-10μm. For copper-plated reinforced tape, the copper plating thickness on one side is 10-30μm, and on both sides it reaches 20-60μm.

[0006] During the annealing process of the superconducting tape after the silver layer is plated, the grains of the silver layer will grow again and aggregate in islands, resulting in the leakage of the superconducting layer in some areas of the tape surface, such as Figure 1 As shown. Figure 2 and Figure 3 As shown, by observing under a microscope, it was found Figure 2 The surface of the silver layer with island aggregation Figure 3 There are obvious differences in the surface of the normal silver layer, and the size of these pores is about 0.1 to 1 um. There are also tiny holes in the silver layer that is magnetron sputtered or evaporated on the surface of the superconducting tape, such as Figure 4 As shown in the figure, the diameter of such defect pores is about 1 to 100 um. At the same time, since silver itself has excellent metal ductility, the upper and lower silver layers are prone to adhesion during the process of winding the strip into a disk, resulting in the silver layer on the surface of the superconducting layer being stained off. The size of such defects is about 10 to 500 um, as shown in the figure. Figure 5As shown. The above factors will cause the current mainstream physical vapor deposition silver layer to be unable to form a complete sheath for the superconducting layer. The patent document with publication number CN113089038A discloses a superconducting tape pre-copper plating method, copper plating method and copper plating device. Although the method of the patent document can effectively repair small pores within 1um such as island-like aggregation of the silver layer, it is difficult to complete the repair of the second and third types of large-sized pores, resulting in the superconducting material in the subsequent copper plating process. The acid directly corrodes the superconducting layer, causing damage to the superconducting film layer. Therefore, it is very critical whether the copper plating layer of the roll-to-roll superconducting tape can form a complete sheath structure for the tape before the liquid enters the holes to isolate the corrosion of the superconducting layer by the external environment. During the electroplating process, the solution will enter the superconducting layer through these holes and react with the superconducting layer. Therefore, how to solve this problem becomes very difficult.

[0007] At present, based on the extremely high upper critical field characteristics of the second-generation high-temperature superconductors, high-field magnets and fusion magnets are one of the most important applications of the second-generation high-temperature superconductors. However, the requirements for the engineering current density of the tape for these applications are much higher than those for traditional power applications, so most application solutions use copper plating for reinforcement. These applications are limited by the requirements for magnetic field strength, and compared with the current mainstream superconducting cable technology solutions, the bending performance requirements for the superconducting tape itself are very stringent. On the one hand, due to the requirement for overcurrent protection, it is generally believed that a copper layer with a total thickness of more than 40um needs to be plated to effectively protect the tape, such as Figure 6 However, if the metal film is plated entirely by the physical method of vapor deposition, when the total thickness of the copper layer is 40um on the front and back of the strip, the thickness of the copper layer on the side of the strip is too thin, only less than 10um. Because the internal stress of the film plated by physical vapor deposition is relatively large, it is very easy to delaminate at the same turning radius, such as Figure 7 As shown. At present, in the mainstream second-generation high-temperature superconducting tape application fields at home and abroad, all commercial teams have stated that this type of tape cannot be used, which is also the main reason why physical vapor deposition film layers are not suitable for superconducting tape coating.

[0008] Patent document with publication number CN108342757B discloses a method for preparing a protective layer of a high-temperature superconducting tape by electroplating copper, comprising the following steps: step 1, preparing a copper protective layer on a high-temperature superconducting tape by electroplating copper; step 2, electroplating copper on the back side of the superconducting layer. However, the patent document is still based on the electrochemical copper plating method, which is limited by the scientific law of the copper layer growth principle and still cannot solve the large hole defects that may exist on the surface of the superconducting tape, such as Figure 8As shown. Such defects will cause a large amount of water vapor to condense in the holes of the strip after the low-temperature test process of the high-field magnet or other application device made with the strip, and cannot evaporate in time, eventually causing the strip to be corroded by water vapor for a long time and hydrolyze, losing superconductivity. Subsequent disassembly and analysis of the coil revealed that there were obvious circular traces of water stains on these holes, such as Fig. 9 shown.

[0009] In addition, due to the electrochemical copper plating method, some very small micron-level strip defects on the surface of the silver strip, such as Fig.10 As shown in Figure 2, during electrochemical copper plating, a tip effect is easily formed near the defect, causing the defect to be further enlarged in size after copper plating, such as Fig.11 These become large-sized particle defects, such as Fig.12 As shown in the figure, the strip is easily scratched during the repeated rewinding process, resulting in damage to the film surface, exposing the superconducting layer directly, and then being damaged by deliquescence in the atmospheric environment, such as Fig.13 At the same time, the copper electroplating method will also cause some copper layers grown on silver layer defects to be further amplified in subsequent processing. For example, in the process of scraping tin on the copper-plated strip, since the original copper layer is electroplated on the defective silver layer, the entire copper layer will peel off after scraping tin, as shown in the figure below. Fig.14 shown.

[0010] In summary, copper plating of superconducting tapes faces the above complex technical problems that need to be solved urgently. In addition, the overall price level of second-generation high-temperature superconducting tapes is currently 300 to 400 yuan per meter. However, due to the sensitivity of superconducting applications to joint resistance, most applications require a single strip of 100 meters or more, so strips below 100 meters have almost no commercial value. Various defects on the silver and copper layers will lead to a significant reduction in the effective length of the strip, causing huge economic losses to the production of second-generation high-temperature superconducting tapes. Summary of the invention

[0011] In view of the defects in the prior art, an object of the present invention is to provide a ReBCO protective layer processing method.

[0012] A ReBCO protective layer processing method provided by the present invention comprises the following steps:

[0013] Step 1: Physically coating the superconducting tape to form a protective layer by physical vapor deposition; the coating thickness is less than or equal to 2um, and the coating temperature is less than or equal to 200°C;

[0014] Step 2: chemically copper-plating the physically plated superconducting tape by electroplating copper.

[0015] Preferably, the surface of the superconducting tape is coated on one side or on both sides.

[0016] Preferably, the bending diameter of the prepared superconducting tape can be less than or equal to 5 mm.

[0017] Preferably, in step 1, the superconducting tapes cut into different widths are plated.

[0018] Preferably, the chemical copper plating specifically comprises the following steps:

[0019] Step 2.1: The processed strip is sequentially subjected to a primary cleaning treatment, a bright copper plating treatment, a sand surface copper plating treatment, and then a secondary cleaning treatment;

[0020] Step 2.2: Passivation treatment and drying treatment are performed on the processed strip after the secondary cleaning treatment.

[0021] Preferably, the surface roughness of the sanded copper is greater than 50 nm.

[0022] Preferably, in the step 2.1, a pre-copper plating treatment is performed before the copper plating treatment, the pre-copper plating treatment adopts a first current electroplating treatment, the bright copper plating treatment adopts a third current electroplating treatment, and the sand surface copper plating treatment adopts a second current electroplating treatment.

[0023] Preferably, the current density used by the first current is 6-20 A / dm^2, the current density used by the third current is 0.5-3.5 A / dm^2, and the current density used by the second current is 3-8 A / dm^2.

[0024] Preferably, the pre-copper plating solution used in the pre-copper plating treatment is added with a pre-copper acid additive that allows operation at a current density of 6 to 20 A / dm^2, and the weight composition of the pre-copper plating solution is:

[0025] 200-240 parts of copper sulfate;

[0026] 50-70 parts of sulfuric acid;

[0027] Chloride ion 0.08-0.1 part;

[0028] The bright copper plating solution used in the bright copper plating treatment is added with a bright copper acid copper additive that allows operation at a current density of 0.5 to 3.5 A / dm^2. The weight composition of the bright copper plating solution is:

[0029] 60-100 parts of copper sulfate;

[0030] 170-200 parts of sulfuric acid;

[0031] Chloride ion 0.06-0.09 parts;

[0032] The copper electroplating solution used in the copper plating treatment is added with copper acid additives that allow the copper to work at a current density of 3 to 8 A / dm^2. The copper electroplating solution has a weight composition of:

[0033] 180-220 parts of copper sulfate;

[0034] 50-80 parts of sulfuric acid;

[0035] Chloride ion 0.06-0.13 parts.

[0036] Preferably, the weight composition of the pre-plating acid copper additive is:

[0037] 6 to 8 parts of tank opening agent;

[0038] 2-3 servings of supplement.

[0039] Preferably, in step 1, the coating material is any one of the following: gold, palladium, copper.

[0040] Preferably, in step 1, a copper protective layer is plated on the surface of the superconducting tape.

[0041] Preferably, in step 1, the superconducting tape is asymmetrically copper plated so that the copper layer thickness on the superconducting layer side is greater than the copper layer thickness on the substrate side, or copper is plated only on the superconducting layer side.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1. The present invention combines physical copper plating with chemical copper plating to make the prepared superconducting tape have good bending properties without delamination.

[0044] 2. The present invention firstly uses physical copper plating to solve the problem that some random fine pores are generated on the surface due to the thinness of the silver-plated superconducting tape layer, and the pores caused by the island aggregation effect caused by annealing, especially some pores with a diameter greater than 1um, are easily corroded by electroplated copper acid solution.

[0045] 3. The present invention firstly uses physical copper plating to solve the problem that after the silver-plated superconducting tape is wound into a roll, the silver layer sticks to the upper and lower parts, resulting in the superconducting layer in some areas being exposed and easily corroded by the electroplated copper acid solution.

[0046] 4. The present invention first solves the problem of electrochemical copper plating having strict requirements on the uniformity of the surface conductivity of the silver layer by physical copper plating, so that part of the silver layer cannot be plated with copper or the bonding force between the copper layer and the silver layer is very weak, and part of the copper layer is very easy to fall off, resulting in pores with silver but no copper on the surface of the strip.

[0047] 5. The present invention solves the problem that fine particles on the surface of the silver strip are further amplified due to the tip effect of electroplating during the copper electroplating process by physical copper plating.

[0048] 6. The present invention uses physical copper plating to solve the problem of uneven electroplating caused by the difference between the front and rear tanks on the surface of the strip in multiple electroplating tanks during the roll-to-roll parallel plating process.

[0049] 7. The present invention first performs physical copper plating to form a structure in which a copper layer completely covers the surface of the superconducting tape, and then performs chemical copper plating, thereby avoiding the defects on the surface of the silver layer of the superconducting tape being affected by acid during copper plating and damaging the film layer.

[0050] 8. The present invention performs physical plating first and then chemical copper plating, thereby preventing the superconducting layer from being damaged during subsequent processing and use due to defects on the surface of the silver tape. At the same time, it also solves the defects of excessive internal stress in the film layer and easy delamination of the tape when relying solely on physical vapor deposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0052] Figure 1 Schematic diagram of the island-like aggregation and fine pores on the surface of the silver ribbon after the annealing process;

[0053] Figure 2 A schematic diagram of the surface of the silver layer with island-like aggregation under a microscope;

[0054] Figure 3 It is a schematic diagram of the normal silver layer surface under a microscope;

[0055] Figure 4 A schematic diagram showing the tiny pores on the surface of the silver layer of a superconducting tape;

[0056] Figure 5 A schematic diagram showing the adhesion of the silver layer between the upper and lower layers of the silver-plated tape;

[0057] Figure 6 Schematic diagram of the cross section of a superconducting tape with a total thickness of copper-plated reinforced copper layer greater than 40um;

[0058] Figure 7 This is a schematic diagram of the delamination of the strip after bending due to excessive stress in the film layer during physical vapor deposition copper plating;

[0059] Figure 8 A schematic diagram showing the defects of the silver layer leaking from the pores of the copper layer on the surface of the superconducting tape after physical copper plating;

[0060] Fig. 9A schematic diagram showing the circular traces of obvious water corrosion on the superconducting layer at the pores;

[0061] Fig.10 A schematic diagram showing defects in superconducting silver ribbons;

[0062] Fig.11 A schematic diagram showing the defects of the silver strip of the superconducting strip after electrochemical copper plating;

[0063] Fig.12 A schematic diagram showing the particles on the surface of the copper-plated superconducting tape;

[0064] Fig.13 A schematic diagram showing the superconducting layer exposed after the copper-plated particles on the surface of the superconducting tape are scratched;

[0065] Fig.14 A schematic diagram showing the peeling of the entire copper layer after the superconducting tape is tinned;

[0066] Fig.15 is a flow chart of the steps of the ReBCO protective layer processing method of the present invention;

[0067] Fig.16 A schematic diagram showing that the superconducting tape prepared by the ReBCO protective layer processing method of the present invention does not delaminate after bending;

[0068] Fig.17 Schematic diagram showing that small particles on the surface of the silver strip do not grow larger due to the tip effect during the electrochemical copper plating process. DETAILED DESCRIPTION

[0069] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0070] Embodiment 1:

[0071] like Fig.15 As shown, this embodiment provides a ReBCO protective layer processing method, including the following steps:

[0072] Step 1: Physically coat the superconducting tape with a protective layer by physical vapor deposition; the thickness of the coating on one side is less than or equal to 2um, and the vacuum of the body reaches 1*10 -6T, coating temperature 200℃; using a tape speed of 200m / h, a vacuum chamber pressure of 5-8mt, a magnetron target power of 1000W, and a coating process with a target distance of 7cm, the superconducting tapes cut into different widths are coated; the surface of the superconducting tape is coated on one side or on both sides; the protective layer is a metal layer.

[0073] Step 2: chemically copper-plating the physically plated superconducting tape by electroplating copper; chemical copper plating specifically includes the following steps:

[0074] Step 2.1: The processed strip is subjected to a belt running speed of 200 m / h, and is sequentially subjected to a cleaning treatment, a bright copper plating treatment, a sand surface copper plating treatment, and then a secondary cleaning treatment; the surface roughness of the sand surface copper is greater than 50 nm; a pre-copper plating treatment is first performed before the copper plating treatment, the pre-copper plating treatment adopts a first current electroplating treatment, the bright copper plating treatment adopts a third current electroplating treatment, and the sand surface copper plating treatment adopts a second current electroplating treatment; the current density adopted by the first current is 6 to 20 A / dm^2, the current density adopted by the third current is 0.5 to 3.5 A / dm^2, and the current density adopted by the second current is 3 to 8 A / dm^2; a pre-plating acid copper additive that allows a current density of 6 to 20 A / dm^2 to be added to the pre-copper plating solution adopted in the pre-copper plating treatment, and the weight composition of the pre-copper plating solution is: 200 to 240 parts of copper sulfate; 50 to 70 parts of sulfuric acid; 0.08 to 0.1 parts of chloride ions. The bright copper plating treatment uses a bright copper acid copper additive that allows a current density of 0.5 to 3.5 A / dm^2. The weight composition of the bright copper plating solution is: 60 to 100 parts of copper sulfate; 170 to 200 parts of sulfuric acid; 0.06 to 0.09 parts of chloride ions. The sand surface copper plating treatment uses a sand surface copper plating solution that allows a current density of 3 to 8 A / dm^2. The weight composition of the sand surface copper plating solution is: 180 to 220 parts of copper sulfate; 50 to 80 parts of sulfuric acid; 0.06 to 0.13 parts of chloride ions. The weight composition of the pre-plating acid copper additive is: 6 to 8 parts of a cylinder opening agent; 2 to 3 parts of a supplement.

[0075] Step 2.2: After the secondary cleaning, the processed strip is passivated and dried at 200 m / h.

[0076] The bending diameter of the prepared superconducting tape can be less than or equal to 5 mm; the single-side thickness of the prepared superconducting tape is less than or equal to 5 um;

[0077] In this embodiment, physical plating is first performed to form a metal layer shielding structure on the surface of the superconducting tape and then copper electroplating is performed, thereby effectively avoiding the corrosion of the defective parts of the silver layer by the copper electroplating acid solution.

[0078] Embodiment 2:

[0079] Those skilled in the art may understand this embodiment as a more specific description of Embodiment 1.

[0080] like Fig.15 As shown, this embodiment provides a roll-to-roll superconducting tape copper plating method, comprising the following steps:

[0081] Step 1: Physical copper plating of superconducting tape by physical vapor deposition; asymmetric copper plating of superconducting tape, the bulk vacuum reaches 1*10 -6 T, coating temperature 200 ° C, the superconducting surface is equipped with a tape speed of 200 m / h, the vacuum chamber pressure is 5-8 mt, the magnetron target power is 1000 W, and the coating process with a target distance of 7 cm is adopted. For the non-superconducting surface, the tape speed is 400 m / h, the vacuum chamber pressure is 5-8 mt, the magnetron target power is 1000 W, and the coating process with a target distance of 7 cm is adopted to make the copper layer thickness on the superconducting layer side greater than the copper layer thickness on the substrate side; or when the bulk vacuum reaches 1*10 -6 T, under the coating temperature of 200℃, the tape speed of 200m / h was used only for the superconducting layer side, the vacuum chamber pressure was 5-8mt, the magnetron target power was 1000W, and the coating process with a target distance of 7cm was used for copper plating.

[0082] Step 2: chemically copper-plating the superconducting tape that has been physically copper-plated by electroplating. The chemical copper-plating step specifically includes the following steps:

[0083] Step 2.1: The processed strip is subjected to a primary cleaning treatment, a bright copper plating treatment, a sand surface copper plating treatment, and a secondary cleaning treatment at 300 m / h; the surface roughness of the sand surface copper is greater than 50 nm.

[0084] Step 2.2: After the secondary cleaning, the processed strip is passivated and dried at 300 m / h.

[0085] In step 2.1, a pre-copper plating treatment is performed before the copper plating treatment. The pre-copper plating treatment adopts a first current electroplating treatment, the bright copper plating treatment adopts a third current electroplating treatment, and the sand surface copper plating treatment adopts a second current electroplating treatment. The current density used by the first current is 6 to 20A / dm^2, the current density used by the third current is 0.5 to 3.5A / dm^2, and the current density used by the second current is 3 to 8A / dm^2.

[0086] The pre-copper plating solution used in the pre-copper plating treatment adds a pre-copper acid additive that allows a current density of 6 to 20 A / dm^2, and the weight composition of the pre-copper plating solution is: 200 to 240 parts of copper sulfate; 50 to 70 parts of sulfuric acid; 0.08 to 0.1 parts of chloride ions. The bright copper plating solution used in the bright copper plating treatment adds a bright copper acid additive that allows a current density of 0.5 to 3.5 A / dm^2, and the weight composition of the bright copper plating solution is: 60 to 100 parts of copper sulfate; 170 to 200 parts of sulfuric acid; 0.06 to 0.09 parts of chloride ions. The sand surface copper plating solution used in the sand surface copper plating treatment adds a sand surface copper acid additive that allows a current density of 3 to 8 A / dm^2, and the weight composition of the sand surface copper plating solution is: 180 to 220 parts of copper sulfate; 50 to 80 parts of sulfuric acid; 0.06 to 0.13 parts of chloride ions. The weight composition of the pre-plating acid copper additive is: 6 to 8 parts of the tank opening agent; and 2 to 3 parts of the supplementing agent.

[0087] The minimum bending diameter of the prepared superconducting tape is less than or equal to 5 mm.

[0088] This embodiment first performs physical plating to form a metal layer shielding structure on the surface of the superconducting tape and then performs electroplating copper, thereby effectively avoiding the corrosion of the defective parts of the silver layer by the electroplating copper acid solution. This embodiment combines physical copper plating with chemical copper plating to make the minimum bending diameter of the prepared superconducting tape less than 5 mm. This embodiment first fills the micropores on the surface of the superconducting tape by physical copper plating, thereby solving the problem that the solution will enter the holes and corrode the superconducting layer during the electrochemical copper plating. This embodiment effectively controls the internal stress of the copper layer of the superconducting tape by chemical copper plating, and solves the technical problems of excessive minimum bending radius of the superconducting tape and easy delamination of the tape caused by physical copper plating. Fig.16 This embodiment effectively covers the defects on the surface of the silver strip by physical copper plating, and greatly suppresses the growth of small particles caused by the presence of sharp particle structures in electrochemical copper plating, such as Fig.17 shown.

[0089] The present invention performs physical copper plating first and then chemical copper plating, thereby avoiding the destruction of the superconducting film layer during copper electroplating due to various defects in the silver tape of the superconducting tape, and solving the problem that the minimum bending radius of the superconducting tape plated by physical vapor phase is too large and it is extremely easy to delaminate during the coil winding process.

[0090] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A ReBCO protective layer processing method, characterized in that: The steps include: Step 1: Physically copper-plating a protective layer on the superconducting tape by physical vapor deposition; the thickness of the coating on one side is less than or equal to 2 μm, and the coating temperature is less than or equal to 200°C; the micropores on the surface of the superconducting tape are filled by physical copper plating; Step 2: chemically copper-plating the superconducting tape that has been physically copper-plated by electroplating copper; The bending diameter of the prepared superconducting tape is less than or equal to 5 mm, so that the prepared superconducting tape has good bending performance and will not have delamination.

2. The ReBCO protective layer processing method according to claim 1, characterized in that: The surface of the superconducting tape is coated on one side or on both sides.

3. The ReBCO protective layer processing method according to claim 1, characterized in that: In the step 1, the superconducting tapes cut into different widths are plated.

4. The ReBCO protective layer processing method according to claim 1, characterized in that: The chemical copper plating specifically comprises the following steps: Step 2.1: The processed strip is sequentially subjected to a primary cleaning treatment, a bright copper plating treatment, a sand surface copper plating treatment, and then a secondary cleaning treatment; Step 2.2: Passivation treatment and drying treatment are performed on the processed strip after the secondary cleaning treatment.

5. The ReBCO protective layer processing method according to claim 4, characterized in that: The surface roughness of the sand-surface copper is greater than 50 nm.

6. The ReBCO protective layer processing method according to claim 4, characterized in that: In the step 2.1, a pre-copper plating treatment is performed before the copper plating treatment, the pre-copper plating treatment adopts a first current electroplating treatment, the bright copper plating treatment adopts a third current electroplating treatment, and the sand surface copper plating treatment adopts a second current electroplating treatment.

7. The ReBCO protective layer processing method according to claim 6, characterized in that: The current density of the first current is 6-20 A / dm 2 The current density of the third current is 0.5-3.5 A / dm 2 The current density of the second current is 3 to 8 A / dm 2 .

8. The ReBCO protective layer processing method according to claim 7, characterized in that: The pre-copper plating solution used in the pre-copper plating treatment contains 6 to 20 A / dm 2 The pre-plating acid copper additive for current density operation, the weight composition of the pre-plating copper electroplating solution is: 200-240 parts of copper sulfate; 50-70 parts of sulfuric acid; Chloride ion 0.08-0.1 part; The bright copper plating treatment uses a bright copper plating solution that allows 0.5 to 3.5 A / dm 2 The bright copper acid copper additive working at current density, the bright copper plating electroplating solution weight composition is: 60-100 parts of copper sulfate; 170-200 parts of sulfuric acid; Chloride ion 0.06-0.09 parts; The copper plating treatment uses a copper electroplating solution that allows 3 to 8 A / dm 2 The copper acid copper additive for Shamian copper plating solution working at current density is composed by weight of: 180-220 parts of copper sulfate; 50-80 parts of sulfuric acid; Chloride ion 0.06-0.13 parts.

9. The ReBCO protective layer processing method according to claim 8, characterized in that: The weight composition of the pre-plating acid copper additive is: 6 to 8 parts of tank opening agent; 2-3 servings of supplement.

Citation Information

Patent Citations

  • A method for preparing a protective layer for high-temperature superconducting tape by electroplating copper.

    CN108342757B

  • Copper pre-plating method, copper plating method and copper plating device for superconducting strip

    CN113089038A

  • Method for preparing high-temperature superconducting strip protection layer through copper electroplating

    CN108342757A

  • Roll-to-roll superconducting strip copper plating device and method

    CN113089060A

  • Copper alloy reinforced superconducting tape, reinforcement method, superconducting coil, and superconducting cable

    CN115171974A