Insulated metal substrate and manufacturing method thereof
By roughening the surfaces of the metal substrate and copper foil, the problem of poor bonding between the metal substrate and the insulating layer in the prior art is solved, and the bonding strength and stability of the insulating metal substrate are improved.
Patent Information
- Application Number
- CN202410243859.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-03-04
Smart Images

Figure CN118158918B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of insulating metal substrates, and in particular relates to an insulating metal substrate and a manufacturing method thereof. Background Art
[0002] Insulated metal substrate is a metal circuit board material with excellent heat dissipation, high mechanical strength and good processing performance. There are two main structures of insulated metal substrate. One structure is copper foil layer, insulating layer metal substrate layer from top to bottom. This kind of insulated metal substrate is a single-sided copper-clad metal substrate. The other structure is copper foil layer, insulating layer, metal substrate layer, insulating layer copper foil layer from top to bottom. This kind of insulated metal substrate is a double-sided copper-clad metal substrate.
[0003] The insulated metal substrate is made of a metal substrate and an insulating layer of copper foil by hot pressing. According to the different metal materials used in the metal substrate, the insulated metal substrate is divided into aluminum-based copper-clad laminate, copper-based copper-clad laminate, iron-based copper-clad laminate, etc. Among them, aluminum-based copper-clad laminate is a very commonly used insulated metal substrate. The invention patent with application number CN202010965311.7 discloses a method for manufacturing an aluminum-based copper-clad laminate, which uses an aluminum-based copper-clad laminate manufacturing device, which includes a base plate, a supporting device and a pressing device: the specific method for using the above-mentioned aluminum-based copper-clad laminate manufacturing device to manufacture an aluminum-based copper-clad laminate is as follows: S1. Equipment detection: Before the equipment is used, the equipment is routinely inspected manually; S2. Material installation: The copper foil is fixed on the pressing device manually, and then the aluminum substrate with glue is placed on the supporting device, and the supporting device adsorbs and fixes the aluminum substrate; S3. Pressing treatment: First, the pressing device feeds the copper foil above the aluminum substrate, and then the pressing device lays the copper foil on the aluminum substrate and presses it, and finally, the supporting device scrapes off the excess glue; S4. Recycling into the warehouse: After step S3 is completed, the aluminum-based copper-clad laminate that has been pressed and formed is taken out from the equipment manually and stored in the warehouse.
[0004] The aluminum-based copper-clad laminate manufacturing method provided by the above patent can also be used on other insulating metal substrates such as copper-based copper-clad laminates and iron-based copper-clad laminates. The manufacturing method provided by the above patent does not roughen the surface of the metal substrate. The metal substrate that has not been roughened has poor surface adhesion, which easily leads to poor bonding between the metal substrate and the insulating layer. Summary of the invention
[0005] The object of the present invention is to provide an insulating metal substrate and a method for manufacturing the same, aiming to improve the problem that the surface of the metal substrate is not roughened in the existing method for manufacturing the insulating metal substrate. The metal substrate that has not been roughened has poor surface adhesion, which easily leads to poor bonding between the metal substrate and the insulating layer.
[0006] In order to achieve the above object, according to a first aspect of the present invention, a method for manufacturing an insulated metal substrate is provided, comprising the following steps:
[0007] S100, roughening the metal substrate: clean the surface of the metal substrate, put it into a low-concentration acid solution to remove the oxide layer on the surface of the metal substrate; then perform alkali washing to remove the acid solution remaining on the surface of the metal substrate due to acid washing, and then wash it with water and put it into a matte solution for matte treatment, so that the surface of the metal substrate has a certain degree of roughness, wash it with water again to remove the residual matte solution, and then dry the metal substrate;
[0008] S200, making a glass fiber cloth prepreg: semi-curing the glass fiber cloth impregnated with the resin to obtain a glass fiber cloth prepreg, wherein the glass fiber cloth in the glass fiber cloth prepreg is surrounded by the resin;
[0009] S300, preparing a copper foil semi-cured resin sheet: coating a layer of resin on the roughened surface of the copper foil, and then performing a semi-curing treatment to form a layer of resin with uniform thickness on the roughened surface of the copper foil to obtain a copper foil semi-cured resin sheet; the copper foil uses electrolytic copper foil, and the preparation method thereof comprises the following steps:
[0010] S1. Preparation of electrolyte: adding the cleaned copper material, pure water and sulfuric acid into a copper dissolving tank, and adding degreased compressed air and water vapor into the tank to generate a copper sulfate solution;
[0011] S2, solution foil production: the prepared copper sulfate solution is filtered through activated carbon and then sent to the foil production system to produce copper foil to obtain raw foil;
[0012] S3, surface treatment: the surface of the original foil is subjected to deoxidation layer treatment, roughening layer treatment, heat-resistant layer treatment and anti-oxidation layer treatment in sequence to obtain a treated copper foil with roughened surface, strong peeling strength and strong anti-oxidation ability;
[0013] S4, product slitting: Use a slitting machine to cut the copper foil to the required product size;
[0014] S400, lamination treatment: lamination treatment of the roughened metal substrate, the glass fiber cloth prepreg sheet and the copper foil clad prepreg resin sheet; the lamination treatment process comprises the following steps:
[0015] Substitute the resin flow difference CLi at different collection time points into the formula , the average difference of resin flow CLJ is calculated;
[0016] Compare the obtained resin flow average difference CLJ with the resin flow average difference threshold CLJy;
[0017] If the resin flow average difference CLJ is greater than or equal to the resin flow average difference threshold CLJy, a resin flow failure signal is generated; at the same time, through the formula , the resin flow failure ratio BL is calculated;
[0018] Substitute the pressure difference CFi at different acquisition time points into the formula , calculate the pressure difference CFJ;
[0019] Compare the obtained pressure mean difference value CFJ with the pressure mean difference threshold value CFJy;
[0020] If the pressure difference CFJ is greater than or equal to the pressure difference threshold CFJy, a pressure failure signal is generated; at the same time, through the formula , calculate the pressure failure ratio BF;
[0021] If both the resin flow failure signal and the pressure failure signal are obtained at the same time, an impact judgment signal is generated; when the impact judgment signal is obtained, the resin flow failure ratio BL and the pressure failure ratio BF are obtained and substituted into the formula In the above equation, the influence judgment value ZY is calculated; where a1 and a2 are both proportional coefficients;
[0022] If the impact judgment value ZY is less than the impact judgment threshold, a pressure impact signal is generated; when the pressure impact signal is obtained, the formula , calculate and obtain the pressure adjustment value ZFt;
[0023] S500, tail processing, storage and warehousing: remove the excess resin squeezed out by the pressing process and store it in the warehouse.
[0024] Furthermore, the resin used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet is any one of phenolic resin, epoxy resin, melamine formaldehyde resin, and polyester resin, and the resin used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet is the same.
[0025] Furthermore, in step S100, the concentration range of the low-concentration acid solution is between 20% and 30%, the acid solution uses nitric acid or sulfuric acid, and is treated at 40-50°C for 2-4 minutes; the metal substrate is alkaline washed using a 10%-20% concentration of sodium hydroxide solution or sodium carbonate solution, and is treated at 40-50°C for 2-4 minutes; the metal substrate is matte treated using a 3%-5% linolenic acid solution, and is treated at 35-55°C for 8-10 minutes.
[0026] Furthermore, the raw foil system includes a raw foil machine, a washing device, a passivation device, a drying device, a winding device and a guiding device. The raw foil machine includes a raw foil tank, a cathode roller and a stripping roller. The inner surface of the raw foil tank is provided with an iridium dioxide-coated titanium plate as an anode. The cathode roller is horizontally arranged, and its lower half roller body is located in the raw foil tank. The stripping roller is arranged on one side of the cathode roller and is located above the raw foil tank. The stripping roller and the cathode roller are arranged in parallel. The stripping roller and the cathode roller are each connected to a variable speed drive device, and the variable speed drive device is used to drive the roller connected thereto to rotate; the washing device includes a washing tank and a washing roller arranged in the washing tank, and the washing roller is connected to a variable speed drive device; the passivation device includes a passivation device. The invention relates to a passivation tank and a passivation roller arranged in the passivation tank, wherein the passivation roller is also connected to a variable speed drive device; the winding device includes a winding roller, which is also connected to a variable speed drive device; the guide device includes a plurality of guide rollers, and guide rollers are arranged between the stripping roller and the washing device, between the washing device and the passivation device, between the passivation device and the drying device, and between the drying device and the winding device; the stripping roller strips the copper foil on the rotating cathode roller and conveys it to the washing roller of the washing device via the guide roller, the copper foil after washing is conveyed to the passivation device via the guide roller, the copper foil after passivation is conveyed to the drying device via the guide roller, the copper foil after drying is conveyed to the winding device via the guide roller, and is wound up by the winding roller of the winding device.
[0027] Furthermore, the oxidation layer removal process is as follows: firstly, the original foil is pickled to remove the oxidation layer on the surface of the original foil, then it is alkaline washed to remove the acid remaining on the surface of the copper foil, then it is washed with water to remove the alkaline remaining on the surface of the copper foil, and finally it is dried.
[0028] Furthermore, the roughening layer treatment includes a first treatment and a second treatment, and the first treatment and the second treatment are both performed using an electrolytic method. In both treatments, the copper foil is used as a cathode, and copper deposition occurs on the surface of the copper foil. The copper foil is washed and dried between the first treatment and the second treatment, and the concentration and temperature of the electrolyte used in the first treatment and the second treatment, as well as the treatment time, are different.
[0029] Furthermore, the heat-resistant layer treatment is to electroplate a layer of other metal on the surface of the copper foil roughening layer so that the copper foil surface is not in direct contact with the resin. The heat-resistant layer treatment can be any one of galvanizing gray treatment, copper-zinc alloy yellow treatment and nickel black treatment.
[0030] Furthermore, the anti-oxidation layer treatment is to form an anti-oxidation film mainly composed of zinc and chromium on the copper foil heat-resistant layer by electroplating to isolate the air; water washing and drying treatments are required between the roughening layer treatment, the heat-resistant layer treatment and the anti-oxidation layer treatment.
[0031] According to a second aspect of the present invention, there is provided an insulated metal substrate manufactured using the above-mentioned method for manufacturing an insulated metal substrate.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The manufacturing method of the insulated metal substrate provided by the present invention roughens the surface of the metal substrate, thereby improving the adhesion of the surface of the metal substrate and ensuring a firm bond between the metal substrate and the insulating layer.
[0034] 2. The manufacturing method of the insulated metal substrate provided by the present invention performs a roughening layer treatment on the surface of the copper foil. The roughening layer treatment makes the copper foil have a roughened surface, improves the adhesion of the copper foil surface, and makes the copper foil and the insulating layer firmly bonded.
[0035] 3. The manufacturing method of the insulated metal substrate provided by the present invention also performs a heat-resistant layer treatment on the surface of the copper foil. The heat-resistant layer treatment makes the surface of the copper foil have a heat-resistant layer, thereby improving the peeling strength of the copper foil on the insulated metal substrate.
[0036] 4. The manufacturing method of the insulated metal substrate provided by the present invention further performs an anti-oxidation layer treatment on the surface of the copper foil. The anti-oxidation layer treatment provides the surface of the copper foil with an anti-oxidation layer, which can isolate the air from the copper foil and improve the anti-oxidation ability of the copper foil.
[0037] 5. Since the surfaces of the metal substrate and the copper foil are roughened, the bonding force between the metal substrate, the copper foil and the insulating layer is improved, and the stability of the insulated metal substrate is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a method flow chart of the method for manufacturing the insulated metal substrate of the present invention;
[0039] Figure 2 is a method flow chart of the method for preparing electrolytic copper foil according to the present invention;
[0040] Figure 3 It is a structural schematic diagram of the foil production system of the present invention;
[0041] Figure 4 It is a structural schematic diagram of an insulating metal substrate according to the present invention;
[0042] Figure 5 is a schematic structural diagram of another insulating metal substrate according to the present invention;
[0043] Figure 6 It is a schematic structural diagram of the copper foil layer of the insulating metal substrate of the present invention;
[0044] Figure 7 It is a flowchart of the lamination process described in the present invention.
[0045] In the figure: 1. Metal substrate layer; 2. Insulation layer; 3. Copper foil layer; 31. Copper foil substrate; 32. Roughening layer; 33. Heat-resistant layer; 34. Anti-oxidation layer; 4. Foil machine; 41. Foil tank; 42. Cathode roller; 43. Peeling roller; 5. Washing device; 6. Passivation device; 7. Drying device; 8. Winding device; 9. Guide device. DETAILED DESCRIPTION
[0046] The following is a further description with reference to the accompanying drawings and specific embodiments:
[0047] Example 1
[0048] This embodiment provides a method for manufacturing an insulating metal substrate. Figure 1 As shown, the manufacturing method comprises the following steps:
[0049] S100, roughening the metal substrate: clean the surface of the metal substrate, put it into a 20% sulfuric acid solution, and treat it at 40°C for 4 minutes to remove the oxide layer on the surface of the metal substrate. Then perform alkaline washing to remove the acid solution remaining on the surface of the metal substrate due to acid washing. The metal substrate is alkaline washed with a 10% sodium hydroxide solution at 40°C for 4 minutes. After washing with water, put it into a 35°C 3% linolenic acid solution for matte treatment for 10 minutes, so that the surface of the metal substrate has a certain degree of roughness. Wash it with water again to remove the residual matte solution and then dry the metal substrate.
[0050] S200, making a glass fiber cloth prepreg: prepreg the glass fiber cloth impregnated with resin to obtain a glass fiber cloth prepreg, wherein the glass fiber cloth in the glass fiber cloth prepreg is surrounded by the resin. The resin is any one of phenolic resin, epoxy resin, melamine formaldehyde resin, and polyester resin.
[0051] S300, making copper foil semi-cured resin sheet: coating a layer of resin on the roughened surface of the copper foil, and then performing semi-curing treatment to form a layer of resin with uniform thickness on the roughened surface of the copper foil to obtain a copper foil semi-cured resin sheet. The resin uses any one of phenolic resin, epoxy resin, melamine formaldehyde resin, and polyester resin. In order to make the resins of the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet well compatible during hot pressing, the resins used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet should be the same.
[0052] S400, lamination treatment: laminating the roughened metal substrate, the glass fiber cloth prepreg sheet and the copper foil clad prepreg resin sheet.
[0053] S500, tail processing, storage and warehousing: remove the excess resin squeezed out by the pressing process and store it in the warehouse.
[0054] Example 2
[0055] This embodiment provides a method for manufacturing an insulating metal substrate. Figure 1 As shown, the manufacturing method comprises the following steps:
[0056] S100, roughening the metal substrate: clean the surface of the metal substrate, put it into a 20% sulfuric acid solution, and treat it at 50°C for 2 minutes to remove the oxide layer on the surface of the metal substrate. Then perform alkaline washing to remove the acid solution remaining on the surface of the metal substrate due to acid washing. The metal substrate is alkaline washed with a 10% sodium carbonate solution at 50°C for 2 minutes. After washing with water, put it into a 55°C 5% linolenic acid solution for matte treatment for 8 minutes, so that the surface of the metal substrate has a certain degree of roughness. Wash it with water again to remove the residual matte solution and then dry the metal substrate.
[0057] S200, making a glass fiber cloth prepreg: prepreg the glass fiber cloth impregnated with resin to obtain a glass fiber cloth prepreg, wherein the glass fiber cloth in the glass fiber cloth prepreg is surrounded by the resin. The resin is any one of phenolic resin, epoxy resin, melamine formaldehyde resin, and polyester resin.
[0058] S300, making copper foil semi-cured resin sheet: coating a layer of resin on the roughened surface of the copper foil, and then performing semi-curing treatment to form a layer of resin with uniform thickness on the roughened surface of the copper foil to obtain a copper foil semi-cured resin sheet. The resin uses any one of phenolic resin, epoxy resin, melamine formaldehyde resin, and polyester resin. In order to make the resins of the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet well compatible during hot pressing, the resins used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet should be the same.
[0059] In step S300, the copper foil used is electrolytic copper foil, and its preparation method is as follows Figure 2 As shown, the following steps are included:
[0060] S1. Preparation of electrolyte: Add the cleaned copper material, pure water and sulfuric acid into the copper dissolving tank, and add degreased compressed air and water vapor into the tank to generate copper sulfate solution. Compressed air has the dual effects of pressurization and stirring, and water vapor is used to heat the solution. Compressed air must be degreased, otherwise it will increase the pollution of copper sulfate solution.
[0061] S2, solution foil production: the copper sulfate solution is filtered through activated carbon and then sent to the foil production system to produce copper foil to obtain raw foil. Figure 3As shown, the raw foil system includes a raw foil machine 4, a washing device 5, a passivation device 6, a drying device 7, a winding device 8 and a guide device 9. The raw foil machine 4 includes a raw foil tank 41, a cathode roller 42 and a stripping roller 43. The inner surface of the raw foil tank 41 is provided with an iridium dioxide coated titanium plate as an anode. The cathode roller 42 is arranged horizontally, and its lower half roller body is located in the raw foil tank 41. The stripping roller 43 is arranged on one side of the cathode roller 42 and is located above the raw foil tank 41. The stripping roller 43 and the cathode roller 42 are arranged in parallel. The stripping roller 43 and the cathode roller 42 are each connected to a variable speed drive device, and the variable speed drive device is used to drive the roller connected thereto to rotate. The washing device 5 includes a washing tank and a washing roller arranged in the washing tank, and the washing roller is connected to a variable speed drive device. The passivation device 6 includes a passivation tank and a passivation roller arranged in the passivation tank, and the passivation roller is also connected to a variable speed drive device. The winding device 8 includes a winding roller, and the winding roller is also connected to a variable speed drive device. Each variable speed drive device includes a variable frequency motor and a reducer. The variable frequency motor can adjust the speed as needed to adapt to the foil production process. The guide device 9 includes a plurality of guide rollers. Guide rollers are arranged between the stripping roller 43 and the water washing device 5, between the water washing device 5 and the passivation device 6, between the passivation device 6 and the drying device 7, and between the drying device 7 and the winding device 8. The copper sulfate solution in the foil production tank 41 should partially cover the cathode roller 42. When the foil production machine 4 is powered on, the anions hydroxide and sulfate in the anode tank run to the anode made of iridium dioxide coated titanium plate, obtain electrons and are reduced, and the cationic copper ions and hydrogen ions run to the cathode roller of the cathode, lose electrons and are oxidized, and the copper ions are oxidized to copper and adsorbed on the cathode roller. The stripping roller 43 strips the copper foil adsorbed on the rotating cathode roller 42 and transports it to the washing roller of the washing device 5 via the guide roller. The copper foil after washing is transported to the passivation device 6 via the guide roller. The copper foil after passivation is transported to the drying device 7 via the guide roller. The copper foil after drying is transported to the winding device 8 via the guide roller and is wound by the winding roller of the winding device 8. The electrolyte on the surface of the copper foil can be cleaned by washing, the surface of the copper foil is not easily oxidized and corroded by passivation, and the surface of the copper foil is kept dry by drying. The raw foil system can obtain a clean, dry and highly anti-oxidation raw foil.
[0062] S3, surface treatment: the surface of the original foil is sequentially treated with a deoxidation layer, a roughening layer, a heat-resistant layer and an anti-oxidation layer to obtain the following Figure 6The copper foil after treatment with roughened surface, strong peeling strength and strong oxidation resistance is shown. During the storage process, even if the original foil has been dried and passivated, an oxide layer may be generated on the surface. Before the roughening layer treatment, the oxide layer on the surface of the original foil must be removed. The process of removing the oxide layer is as follows: first, the original foil is acid-washed to remove the oxide layer on the surface of the original foil, then the acid solution remaining on the surface of the copper foil is removed by alkali washing, and then the alkali solution remaining on the surface of the copper foil is removed by water washing, and finally drying is performed. The roughening layer treatment includes the first treatment and the second treatment. The first treatment and the second treatment are both carried out by electrolysis. In both treatments, the copper foil is used as the cathode, and copper deposition occurs on the surface of the copper foil. The copper foil is washed and dried between the first treatment and the second treatment. The first treatment and the second treatment can use a mixed solution of copper sulfate solution and sulfuric acid solution, and the mixed solution should have a low copper content and a high acid content. The concentration, temperature and treatment time of the electrolyte used in the first treatment and the second treatment are different. After the first treatment, some copper nodules will form on the surface of the copper foil, but these copper nodules are weakly bonded to the surface of the copper foil and are easy to fall off. After the second treatment, the copper nodules generated are different because the concentration and temperature of the electrolyte used in the two treatments and the treatment time are different. The second copper nodules will fix the first copper nodules so that they will not fall off the copper foil. The heat-resistant layer treatment is to electroplate a layer of other metals on the surface of the roughening layer of the copper foil so that the surface of the copper foil is not in direct contact with the resin. The heat-resistant layer treatment can be any of the galvanized gray treatment, copper-zinc alloy yellow treatment and nickel-plated black treatment. The anti-oxidation layer treatment is to form an anti-oxidation film with zinc and chromium as the main body on the heat-resistant layer of the copper foil by electroplating to isolate the air. Water washing and drying are required between the roughening layer treatment, heat-resistant layer treatment and anti-oxidation layer treatment.
[0063] S4. Product slitting: Use a slitting machine to cut the copper foil into the required product size. After slitting, it will be used in subsequent processes.
[0064] S400, lamination treatment: laminating the roughened metal substrate, the glass fiber cloth prepreg sheet and the copper foil clad prepreg resin sheet.
[0065] S500, tail processing, storage and warehousing: remove the excess resin squeezed out by the pressing process and store it in the warehouse.
[0066] The manufacturing method of the insulated metal substrate provided by the present invention performs a roughening treatment on the surface of the metal substrate, thereby improving the adhesion of the surface of the metal substrate, so that the metal substrate and the insulating layer are firmly bonded. In addition, the manufacturing method of the insulated metal substrate provided by the present invention also performs a roughening layer treatment, a heat-resistant layer treatment and an anti-oxidation layer treatment on the surface of the copper foil. The roughening layer treatment makes the copper foil have a roughened surface, improves the adhesion of the surface of the copper foil, and makes the copper foil and the insulating layer firmly bonded. The heat-resistant layer treatment makes the surface of the copper foil have a heat-resistant layer, which improves the peeling strength of the copper foil on the insulated metal substrate. The anti-oxidation layer treatment makes the surface of the copper foil have an anti-oxidation layer, which can isolate the air from the copper foil and improve the anti-oxidation ability of the copper foil.
[0067] Example 3
[0068] This embodiment provides an insulating metal substrate, which is manufactured using the manufacturing method of the insulating metal substrate provided in Embodiment 2. Figure 4 As shown, the insulated metal substrate includes a three-layer structure, which is a copper foil layer 3, an insulating layer 2 and a metal substrate layer 1 from top to bottom, wherein the copper foil layer 3 includes a copper foil matrix 31, a roughening layer 32, a heat-resistant layer 33 and an anti-oxidation layer 34. The metal substrate layer 1 uses an aluminum plate, and the insulating layer 2 includes a glass fiber cloth and a resin including the glass fiber cloth, and the resin includes a resin of a glass fiber cloth semi-cured sheet and a resin of a copper foil-clad semi-cured resin sheet. The resin uses any one of phenolic resin, epoxy resin, melamine formaldehyde resin and polyester resin. Since the surfaces of the metal substrate and the copper foil are roughened, the bonding force between the metal substrate and the copper foil and the insulating layer 2 is improved, and the stability of the insulated metal substrate is improved.
[0069] Example 4
[0070] This embodiment provides an insulating metal substrate, which is manufactured using the manufacturing method of the insulating metal substrate provided in Embodiment 2. Figure 5 As shown, the insulated metal substrate includes a five-layer structure, which is a copper foil layer 3, an insulating layer 2, a metal substrate layer 1, an insulating layer 2 and a copper foil layer 3 from top to bottom, wherein the copper foil layer 3 includes a copper foil matrix 31, a roughening layer 32, a heat-resistant layer 33 and an anti-oxidation layer 34. The metal substrate layer 1 uses an aluminum plate, and the insulating layer 2 includes a glass fiber cloth and a resin including the glass fiber cloth, and the resin includes a resin of a glass fiber cloth semi-cured sheet and a resin of a copper foil-clad semi-cured resin sheet. The resin uses any one of phenolic resin, epoxy resin, melamine formaldehyde resin and polyester resin. Since the surfaces of the metal substrate and the copper foil are roughened, the bonding force between the metal substrate and the copper foil and the insulating layer 2 is improved, and the stability of the insulated metal substrate is improved.
[0071] Example 5
[0072] like Figure 7As shown, in S400, the pressing process, the pressing process includes the following steps:
[0073] S4001, obtaining resin flow values at different collection time points during lamination, marked as resin flow values ZLi, i represents the collection time point, i=1, 2, 3, ..., n, n is a positive integer, performing difference calculation between the obtained resin flow value ZLi and the resin flow standard value required by the process, and taking the absolute value to obtain the resin flow difference CLi at different collection time points;
[0074] Substitute the resin flow difference CLi obtained at different collection time points into the formula , the average difference of resin flow CLJ is calculated;
[0075] Compare the obtained resin flow average difference CLJ with the resin flow average difference threshold CLJy;
[0076] If the resin flow average difference CLJ is greater than or equal to the resin flow average difference threshold CLJy, a resin flow failure signal is generated; at the same time, through the formula , the resin flow failure ratio BL is calculated;
[0077] If the resin flow average difference CLJ is less than the resin flow average difference threshold CLJy, a resin flow qualified signal is generated;
[0078] S4002, obtaining the pressure values at different acquisition time points during pressing, marked as pressure value ZFi, i represents the acquisition time point, i=1, 2, 3, ..., n, n is a positive integer, calculating the difference between the obtained pressure value ZFi and the pressure standard value required by the process, and taking the absolute value to obtain the pressure difference CFi at different acquisition time points;
[0079] Substitute the pressure difference CFi obtained at different acquisition time points into the formula , calculate the pressure difference CFJ;
[0080] Compare the obtained pressure mean difference value CFJ with the pressure mean difference threshold value CFJy;
[0081] If the pressure difference CFJ is greater than or equal to the pressure difference threshold CFJy, a pressure failure signal is generated; at the same time, through the formula , calculate the pressure failure ratio BF;
[0082] If the pressure difference CFJ is less than the pressure difference threshold CFJy, a tree pressure qualified signal is generated;
[0083] S4003, combining and analyzing the obtained resin flow failure signal, resin flow success signal, pressure failure signal, and pressure success signal;
[0084] If both the resin flow qualified signal and the pressure qualified signal are obtained at the same time, a pressing normal signal is generated;
[0085] If both the resin flow failure signal and the pressure pass signal are obtained at the same time, a pressing inspection signal is generated. When the pressing inspection signal is obtained, the pressing temperature mean TJ during the pressing process is obtained, and the obtained temperature mean TJ is compared with the temperature range value. If the temperature mean TJ is within the temperature range value, a continue inspection signal is generated, and the resin material can be inspected. If the temperature mean TJ is not within the temperature range value, a temperature adjustment signal is generated. By the formula , calculate and obtain the pressing temperature adjustment value ZTt;
[0086] If both the resin flow qualified signal and the pressure unqualified signal are obtained at the same time, a pressure adjustment signal is generated. When the pressure adjustment signal is obtained, the pressure mean value FJ during the pressing process is obtained, and the formula , calculate and obtain the pressure adjustment value ZFt;
[0087] If both the resin flow failure signal and the pressure failure signal are obtained at the same time, an impact judgment signal is generated; when the impact judgment signal is obtained, the resin flow failure ratio BL and the pressure failure ratio BF are obtained and substituted into the formula In the calculation, the influence judgment value ZY is obtained; wherein a1 and a2 are both proportional coefficients, a1 is 0.85, and a2 is 0.16;
[0088] Compare the obtained impact judgment value ZY with the impact judgment threshold;
[0089] If the influence judgment value ZY is greater than or equal to the influence judgment threshold, other influence signals are generated; when other influence signals are obtained, other factors in the pressing process are checked, such as temperature, resin material, etc.; specifically, the pressing temperature mean TJ in the pressing process is obtained, and the obtained temperature mean TJ is compared with the temperature range value. If the temperature mean TJ is within the temperature range value, a continue inspection signal is generated, and the resin material, etc. can be inspected. If the temperature mean TJ is not within the temperature range value, a temperature adjustment signal is generated. By formula , calculate and obtain the pressing temperature adjustment value ZTt;
[0090] If the impact judgment value ZY is less than the impact judgment threshold, a pressure impact signal is generated; when the pressure impact signal is obtained, it can be calculated by the formula , calculate and obtain the pressure adjustment value ZFt;
[0091] The present invention analyzes and judges the resin flow and pressure pressing conditions of the pressing process, realizes real-time monitoring of important influencing factors in the pressing process, ensures the quality of the pressing process, and thus effectively improves the qualified rate of products. In the event of unqualified products, the cause of the failure is analyzed and found, and the corresponding adjustment is completed to ensure the quality of subsequent pressing processes.
[0092] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for manufacturing an insulated metal substrate, characterized in that: The following steps are involved: S100, roughening the metal substrate: cleaning the surface of the metal substrate, placing it in a low-concentration acid solution, and removing the oxide layer on the surface of the metal substrate; Then, alkaline washing is performed to remove the acid solution remaining on the surface of the metal substrate due to acid washing, and then the metal substrate is placed in a matte solution for matte treatment after water washing, so that the surface of the metal substrate has a certain degree of roughness, and then the metal substrate is dried after water washing again to remove the residual matte solution; S200, making a glass fiber cloth prepreg: performing a prepreg treatment on the glass fiber cloth impregnated with the resin to obtain a glass fiber cloth prepreg, wherein the glass fiber cloth in the glass fiber cloth prepreg is surrounded by the resin; S300, preparing a copper foil semi-cured resin sheet: coating a layer of resin on the roughened surface of the copper foil, and then performing a semi-curing treatment to form a layer of resin with uniform thickness on the roughened surface of the copper foil to obtain a copper foil semi-cured resin sheet; the copper foil uses electrolytic copper foil, and the preparation method thereof comprises the following steps: S1. Preparation of electrolyte: adding the cleaned copper material, pure water and sulfuric acid into a copper dissolving tank, and adding degreased compressed air and water vapor into the tank to generate a copper sulfate solution; S2, solution foil production: the prepared copper sulfate solution is filtered through activated carbon and then sent into the foil production system to produce copper foil to obtain raw foil; S3, surface treatment: the surface of the raw foil is sequentially subjected to oxidation layer removal treatment, roughening layer treatment, heat-resistant layer treatment and anti-oxidation layer treatment to obtain a treated copper foil with a roughened surface, strong peeling strength and strong antioxidant capacity; S4, product slitting: Use a slitting machine to cut the copper foil to the required product size; S400, lamination treatment: lamination treatment of the roughened metal substrate, the glass fiber cloth prepreg sheet and the copper foil clad prepreg resin sheet; the lamination treatment process comprises the following steps: S4001, obtaining resin flow values at different collection time points during lamination, marked as resin flow values ZLi, i represents the collection time point, i=1, 2, 3, ..., n, n is a positive integer, performing difference calculation between the obtained resin flow value ZLi and the resin flow standard value required by the process, and taking the absolute value to obtain the resin flow difference CLi at different collection time points; Substitute the resin flow difference CLi obtained at different collection time points into the formula , the average difference of resin flow CLJ is calculated; Compare the obtained resin flow average difference CLJ with the resin flow average difference threshold CLJy; If the resin flow average difference CLJ is greater than or equal to the resin flow average difference threshold CLJy, a resin flow failure signal is generated; at the same time, through the formula , the resin flow failure ratio BL is calculated; If the resin flow average difference CLJ is less than the resin flow average difference threshold CLJy, a resin flow qualified signal is generated; S4002, obtaining the pressure values at different acquisition time points during pressing, marked as pressure value ZFi, i represents the acquisition time point, i=1, 2, 3, ..., n, n is a positive integer, calculating the difference between the obtained pressure value ZFi and the pressure standard value required by the process, and taking the absolute value to obtain the pressure difference CFi at different acquisition time points; Substitute the pressure difference CFi obtained at different acquisition time points into the formula , calculate the pressure difference CFJ; Compare the obtained pressure mean difference value CFJ with the pressure mean difference threshold value CFJy; If the pressure difference CFJ is greater than or equal to the pressure difference threshold CFJy, a pressure failure signal is generated; at the same time, through the formula , calculate the pressure failure ratio BF; If the pressure difference CFJ is less than the pressure difference threshold CFJy, a tree pressure qualified signal is generated; S4003, combining and analyzing the obtained resin flow failure signal, resin flow success signal, pressure failure signal, and pressure success signal; If both the resin flow qualified signal and the pressure qualified signal are obtained at the same time, a pressing normal signal is generated; If both the resin flow failure signal and the pressure pass signal are obtained at the same time, a pressing inspection signal is generated. When the pressing inspection signal is obtained, the pressing temperature mean TJ during the pressing process is obtained, and the obtained temperature mean TJ is compared with the temperature range value. If the temperature mean TJ is within the temperature range value, a continue inspection signal is generated to inspect the resin material. If the temperature mean TJ is not within the temperature range value, a temperature adjustment signal is generated. , calculate and obtain the pressing temperature adjustment value ZTt; If both the resin flow qualified signal and the pressure unqualified signal are obtained at the same time, a pressure adjustment signal is generated. When the pressure adjustment signal is obtained, the pressure mean value FJ during the pressing process is obtained, and the formula , calculate and obtain the pressure adjustment value ZFt; If both the resin flow failure signal and the pressure failure signal are obtained at the same time, an impact judgment signal is generated; when the impact judgment signal is obtained, the resin flow failure ratio BL and the pressure failure ratio BF are obtained and substituted into the formula In the calculation, the influence judgment value ZY is obtained; wherein a1 and a2 are both proportional coefficients, a1 is 0.85, and a2 is 0.16; Compare the obtained impact judgment value ZY with the impact judgment threshold; If the impact judgment value ZY is greater than or equal to the impact judgment threshold, other impact signals are generated; when other impact signals are obtained, other factors in the pressing process are checked, including temperature and resin materials; specifically, the pressing temperature mean TJ in the pressing process is obtained, and the obtained temperature mean TJ is compared with the temperature range value. If the temperature mean TJ is within the temperature range value, a continue inspection signal is generated to inspect the resin material. If the temperature mean TJ is not within the temperature range value, a temperature adjustment signal is generated. By formula , calculate and obtain the pressing temperature adjustment value ZTt; If the impact judgment value ZY is less than the impact judgment threshold, a pressure impact signal is generated; when the pressure impact signal is obtained, the formula , calculate and obtain the pressure adjustment value ZFt; S500, tail processing, storage and warehousing: remove the excess resin squeezed out by the pressing process and store it in the warehouse.
2. The method for manufacturing an insulated metal substrate according to claim 1, characterized in that: The resin used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet is any one of phenolic resin, epoxy resin, melamine formaldehyde resin and polyester resin, and the resin used to make the glass fiber cloth semi-cured sheet and the copper foil semi-cured resin sheet is the same.
3. The method for manufacturing an insulated metal substrate according to claim 1, characterized in that: In the step S100, the concentration range of the low-concentration acid solution is between 20% and 30%, and the acid solution uses nitric acid or sulfuric acid and is treated at 40-50° C. for 2-4 minutes; the metal substrate is alkaline washed using a 10%-20% concentration sodium hydroxide solution or sodium carbonate solution and is treated at 40-50° C. for 2-4 minutes; the metal substrate is matte treated using a 3%-5% linolenic acid solution and is treated at 35-55° C. for 8-10 minutes.
4. The method for manufacturing an insulated metal substrate according to claim 1, characterized in that: The raw foil system comprises a raw foil machine (4), a washing device (5), a passivation device (6), a drying device (7), a winding device (8) and a guiding device (9). The raw foil machine (4) comprises a raw foil trough (41), a cathode roller (42) and a stripping roller (43). The inner surface of the raw foil trough (41) is provided with an iridium dioxide-coated titanium plate as an anode. The cathode roller (42) is arranged horizontally, and its lower half roller body is located in the raw foil trough (41). The stripping roller (43) is arranged on one side of the cathode roller (42) and is located above the raw foil trough (41). The stripping roller (43) and the cathode roller (42) are arranged in parallel. The stripping roller (43) and the cathode roller (42) are respectively connected to a variable speed driving device, and the variable speed driving device is used to drive the rollers connected thereto to rotate. The washing device (5) comprises a washing trough and a washing roller arranged in the washing trough. The washing roller is connected to the variable speed driving device. The passivation device (6) comprises a passivation tank and a passivation roller arranged in the passivation tank, and the passivation roller is also connected to a variable speed drive device; the winding device (8) comprises a winding roller, and the winding roller is also connected to a variable speed drive device; the guide device (9) comprises a plurality of guide rollers, and guide rollers are arranged between the stripping roller (43) and the washing device (5), between the washing device (5) and the passivation device (6), between the passivation device (6) and the drying device (7), and between the drying device (7) and the winding device (8); the stripping roller (43) strips the copper foil on the rotating cathode roller (42) and conveys it to the washing roller of the washing device (5) via the guide roller; the copper foil after washing is conveyed to the passivation device (6) via the guide roller; the copper foil after passivation is conveyed to the drying device (7) via the guide roller; the copper foil after drying is conveyed to the winding device (8) via the guide roller and is wound up by the winding roller of the winding device (8).
5. The method for manufacturing an insulated metal substrate according to claim 1, characterized in that: The oxidation layer removal process is as follows: firstly, the original foil is pickled to remove the oxidation layer on the surface of the original foil, then it is alkali washed to remove the acid remaining on the surface of the copper foil, then it is washed with water to remove the alkali remaining on the surface of the copper foil, and finally it is dried.
6. The method for manufacturing an insulated metal substrate according to claim 5, characterized in that: The roughening layer treatment includes a first treatment and a second treatment, and the first treatment and the second treatment are both performed using an electrolytic method. In both treatments, copper foil is used as a cathode, and copper deposition occurs on the surface of the copper foil. The copper foil is washed and dried between the first treatment and the second treatment, and the concentration and temperature of the electrolyte used in the first treatment and the second treatment, as well as the treatment time, are all different.
7. The method for manufacturing an insulated metal substrate according to claim 6, characterized in that: The heat-resistant layer treatment is to electroplate a layer of other metal on the surface of the copper foil roughening layer so that the copper foil surface does not directly contact the resin. The heat-resistant layer treatment can be any one of galvanizing gray treatment, copper-zinc alloy yellow treatment and nickel black treatment.
8. The method for manufacturing an insulated metal substrate according to claim 7, characterized in that: The anti-oxidation layer treatment is to form an anti-oxidation film mainly composed of zinc and chromium on the copper foil heat-resistant layer by electroplating to isolate the air; water washing and drying treatments are required between the roughening layer treatment, the heat-resistant layer treatment and the anti-oxidation layer treatment.
9. An insulating metal substrate, characterized in that: It is manufactured using the manufacturing method of the insulated metal substrate as described in any one of claims 1 to 8.