A high-efficiency uranium adsorption composite gel material and preparation method thereof

By using the highly efficient adsorption uranium composite gel material prepared by reducing graphene oxide solution and silicon gel mixture, dopamine hydrochloride and acrylonitrile copolymerized, the problems of low adsorption amount, difficulty in separation and high cost are solved, and the adsorbent is achieved. The efficient and low-cost uranium ion adsorption effect significantly improves the efficiency of treating uranium-containing wastewater.

CN118162102BActive Publication Date: 2024-11-26UNIV OF JINAN +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410487212.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-23
Publication Date
2024-11-26
Estimated Expiration
2044-04-23

AI Technical Summary

Technical Problem

The adsorption amount of existing adsorbents is not high, difficult to separate, and costly when treating uranium-containing wastewater, making it difficult to effectively treat nuclear-contaminated wastewater.

Method used

Using highly efficient adsorption uranium composite gel material prepared from reduced graphene oxide solution and silicon gel mixture, dopamine hydrochloride and acrylonitrile copolymerize to form silicon-carbon with high specific surface area and polyhydroxy, carboxyl and epoxy groups. Compound gel to achieve efficient adsorption of uranium ions.

Benefits of technology

It has achieved efficient adsorption of uranium ions, with a maximum adsorption amount of 864ppm and above, which is low in cost, easy to separate and reuse, and does not produce secondary waste, which significantly improves the processing efficiency and resource utilization rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118162102B_ABST
    Figure CN118162102B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid waste material recycling and reuse, in particular to a high-efficiency uranium adsorption composite gel material and a preparation method thereof. The high-efficiency uranium adsorption composite gel material is composed of a reduced graphene oxide solution and a silica gel mixed solution, wherein the silica gel mixed solution is mainly composed of waste wind turbine blade powder and spherical silicon micropowder. The preparation method of the high-efficiency uranium adsorption composite gel material comprises adding the reduced graphene oxide solution to the silica gel mixed solution, stirring at room temperature, filtering, collecting products, washing, and drying to obtain the high-efficiency uranium adsorption composite gel material. The high-efficiency uranium adsorption composite gel material prepared by compounding waste wind turbine blade powder, spherical silicon micropowder and reduced graphene oxide solution has a high adsorption capacity for uranium, a high adsorption selectivity, good reusability, and no secondary waste is generated. The preparation process of the invention is simple, the investment is small, the cost is low, and the adsorbed pollutants are easy to separate and recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid waste material recycling and reuse, in particular to a high-efficiency uranium adsorption composite gel material and a preparation method thereof. Background Art

[0002] With the rapid development of nuclear power worldwide, demand for uranium is increasing. However, the mining and hydrometallurgical processes of uranium ore generate large quantities of uranium-containing wastewater. This wastewater not only pollutes surface water but also seeps into the ground, contaminating groundwater and entering organisms, causing significant harm.

[0003] Research shows that nuclear wastewater contains over 60 radioactive elements. Once discharged into the sea, it poses unpredictable risks to the marine environment and human health. The damage to the surrounding marine ecosystem caused by nuclear wastewater discharge is irreversible. The marine ecosystem is a crucial component of marine resources, and this process will affect the abundance and quality of various organisms and plants.

[0004] Therefore, studying reasonable, safe and effective materials for treating radioactive waste and separating uranium from uranium-containing wastewater can not only improve resource utilization, but also improve nuclear safety and reduce the harm of uranium-containing wastewater to the environment.

[0005] Currently, the main methods for treating uranium-containing wastewater include chemical precipitation, ion exchange, and adsorption. Adsorption has been widely used in the treatment of uranium-containing wastewater due to its low cost, simple process, and low risk of secondary contamination. However, traditional inorganic materials as adsorbents have the disadvantages of low adsorption capacity and difficulty in separation. Furthermore, the cost of preparing adsorbents using traditional inorganic materials is high. Therefore, there is an urgent need to develop a low-cost, high-adsorption, and easily separable adsorbent for treating uranium-containing wastewater. Summary of the Invention

[0006] The present invention aims to solve the shortcomings of existing adsorbents such as low adsorption capacity, difficulty in separation and high cost, and provides an adsorbent material and a preparation method that are easy to separate, have high adsorption capacity and low cost.

[0007] The first object of the present invention is to provide a high-efficiency uranium adsorption composite gel material, which is composed of a reduced graphene oxide solution and a silica gel mixture; the silica gel mixture is mainly composed of waste wind turbine blade powder and spherical silicon powder.

[0008] A second object of the present invention is to provide a method for preparing a composite gel material with high efficiency in uranium adsorption, the method comprising the following steps:

[0009] 1) Preparing a silica gel mixture: 8 g to 15 g of waste wind turbine blade powder and 80 mg to 150 mg of spherical silica powder are mixed, and then added to 150 mL to 250 mL of deionized water. The mixture is stirred at a speed of 150 to 300 rpm for 90 to 150 minutes to prepare a silica gel mixture for later use.

[0010] 2) taking 1-2 parts of the reduced graphene oxide solution and 2-4 parts of the silica gel mixture by weight ratio, adding the reduced graphene oxide solution to the silica gel mixture, and stirring at room temperature for 2-4 hours to prepare a mixture I;

[0011] 3) Filtering the mixed solution I, collecting the product, washing the product with deionized water until the pH value is neutral, and drying the product at 35-45° C. to obtain a high-efficiency uranium adsorption composite gel material.

[0012] Furthermore, the preparation method of the waste wind turbine blade powder is: taking waste wind turbine blades, cutting, crushing, pulverizing, grinding, and screening the waste wind turbine blades to obtain waste wind turbine blade powder.

[0013] Furthermore, the particle size of the waste wind turbine blade powder is about 25 to 100 nm.

[0014] Furthermore, the preparation method of the reduced graphene oxide solution is as follows: 80 mL-150 mL of graphene oxide dispersion and 80 mL-150 mL of alkaline modified solution are taken, the alkaline modified solution is slowly poured into the graphene oxide dispersion, and the reduced graphene oxide solution is prepared by water bathing at 50° C.-70° C. for 22 to 26 hours.

[0015] Furthermore, the preparation method of the alkaline modified solution is:

[0016] 1) Dissolve 2.2 mol to 2.8 mol of Tris in 80 mL to 150 mL of deionized water, and stir magnetically until the Tris is completely dissolved to prepare a Tris mixture;

[0017] 2) adding a tris(hydroxymethyl)aminomethane (Tris) mixed solution to the modified solution to obtain a mixed solution II;

[0018] 3) The pH value of the mixed solution II is then adjusted to 8.5 to obtain an alkaline modified solution.

[0019] Furthermore, the preparation method of the modified solution is:

[0020] 1) Add 130 mL to 180 mL of deionized water and 170 mL to 250 mL of ethanol by volume, and stir at 150 to 300 rpm for 10 to 15 minutes to prepare a mixed solution III.

[0021] 2) Add 1.5 mol-4 mol of dopamine hydrochloride and 0.2 mol-1 mol of acrylonitrile to the mixed solution III, and stir for 10-15 minutes at a rotation speed of 150-300 r / min to prepare a modified solution.

[0022] The beneficial effects of the present invention are:

[0023] The invention belongs to the technical field of solid waste material recycling and reuse, and discloses a method for preparing a high-efficiency uranium adsorption composite gel material by compounding discarded wind turbine blade powder, spherical silicon micropowder and reduced graphene oxide solution.

[0024] The present invention utilizes copolymerization of dopamine hydrochloride and acrylonitrile to modify a silicon-carbon composite gel. This allows the highly efficient uranium adsorption composite gel to fully adsorb uranium ions on the surface of spherical silicon micropowder upon contact with the spherical silicon micropowder, thereby preparing ultrapure spherical silicon micropowder. The copolymerization of dopamine hydrochloride and acrylonitrile results in the production of more hydrophilic groups, while graphene oxide possesses a higher specific surface area and numerous carboxyl, hydroxyl, and epoxy groups. This results in the formation of a denser nanofilm within the pores of the silicon-carbon composite gel, which can both undergo complexation reactions with heavy metal ions and interact with organic pollutants, resulting in a higher adsorption rate.

[0025] The preparation process described in this invention is simple and reuses renewable resources, such as waste wind turbine blade powder. This approach requires minimal investment and is cost-effective. Adsorbed pollutants can be easily separated and recovered, laying the foundation for the high-value-added secondary utilization of waste wind turbine blades. Related tests have shown that the material of this invention has a high adsorption capacity for uranium and exhibits high adsorption selectivity, high reusability, and no secondary waste.

[0026] The maximum adsorption capacity of the high-efficiency uranium adsorption composite gel material prepared by the present invention reaches about 864 ppm or above. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Microscopic morphologies of composite gel (a), graphene oxide (b), graphene oxide-composite gel (c), and PDA and acrylonitrile modified graphene-composite gel (d);

[0028] Figure 2 The infrared spectra of composite gel, graphene oxide, graphene oxide-composite gel and PDA and acrylonitrile modified graphene-composite gel;

[0029] Figure 3 This is a diagram showing the adsorption effect of uranium standard solution, composite gel, PDA and acrylonitrile-modified graphene-composite gel on uranium. DETAILED DESCRIPTION

[0030] In order to better understand the present invention, the technical solutions of the present invention are described in detail below with specific examples, but the present invention is not limited thereto.

[0031] The waste wind turbine blades used in the present invention are selected from the Jiuquan Wind Power Base in Gansu Province (a 10 million kilowatt wind power base located in Jiuquan City, Gansu Province, and the first 10 million kilowatt wind power base in China).

[0032] Other raw materials used in the present invention are all commercially available products.

[0033] Example 1 A high-efficiency uranium adsorption composite gel material and its preparation method

[0034] A highly efficient uranium adsorption composite gel material consists of a reduced graphene oxide solution and a silica gel mixture, wherein the silica gel mixture mainly consists of waste wind turbine blade powder and spherical silica powder.

[0035] The specific steps are as follows:

[0036] Step 1: Preparation of waste wind turbine blade powder:

[0037] Taking waste wind turbine blades, cutting, crushing, pulverizing, grinding, and screening the waste wind turbine blades to obtain waste wind turbine blade powder, wherein the particle size of the waste wind turbine blade powder is about 25 nm, and the waste wind turbine blade powder is set aside;

[0038] Step 2: Prepare the modified solution:

[0039] 1) Take 150 mL of deionized water and 200 mL of ethanol by volume, add the deionized water to the ethanol, and stir at 300 r / min for 10 minutes to prepare mixed solution III;

[0040] 2) Add 2.5 mol of dopamine hydrochloride and 0.5 mol of acrylonitrile to the mixed solution III, and stir at a speed of 300 r / min for 10 minutes to prepare a modified solution for later use;

[0041] Step 3: Prepare alkaline modified solution:

[0042] 1) Dissolve 2.5 mol of Tris in 100 mL of deionized water and stir magnetically until the Tris is completely dissolved to prepare a Tris mixture;

[0043] 2) adding a tris(hydroxymethyl)aminomethane (Tris) mixed solution to the modified solution to obtain a mixed solution II;

[0044] 3) The pH value of the mixed solution II is then adjusted to 8.5 to obtain an alkaline modified solution;

[0045] Step 4: Prepare a reduced graphene oxide solution: Take 100 mL of graphene oxide dispersion and 100 mL of alkaline modified solution, slowly pour the alkaline modified solution into the graphene oxide dispersion, and incubate in a water bath at 60° C. for 24 hours to prepare a reduced graphene oxide solution;

[0046] Step 5: Prepare a silica gel mixture: Take 10 g of waste wind turbine blade powder and 100 mg of spherical silica powder, add the wind turbine blade powder and spherical silica powder to 200 mL of deionized water, and stir at a speed of 300 r / min for 120 minutes to prepare a silica gel mixture;

[0047] Step 6: Preparation of high-efficiency uranium adsorption composite gel material:

[0048] 1) adding 1 part of the reduced graphene oxide solution to 2 parts of the silica gel mixture in a mass ratio, stirring at room temperature for 3 hours to prepare a mixture I;

[0049] 2) The mixed solution I is filtered to collect the product, which is then washed with deionized water until the pH value is neutral, and then dried at 40° C. to obtain a composite gel material with high efficiency in adsorbing uranium.

[0050] Example 2 A high-efficiency uranium adsorption composite gel material and its preparation method

[0051] A highly efficient uranium adsorption composite gel material consists of a reduced graphene oxide solution and a silica gel mixture, wherein the silica gel mixture mainly consists of waste wind turbine blade powder and spherical silica powder.

[0052] The specific steps are as follows:

[0053] Step 1: Preparation of waste wind turbine blade powder:

[0054] Taking waste wind turbine blades, cutting, crushing, pulverizing, grinding, and screening the waste wind turbine blades to obtain waste wind turbine blade powder, wherein the particle size of the waste wind turbine blade powder is about 50 nm, and the waste wind turbine blade powder is set aside;

[0055] Step 2: Prepare the modified solution:

[0056] 1) 130 mL of deionized water and 170 mL of ethanol were added to the ethanol by volume, and the mixture was stirred at 200 r / min for 13 minutes to prepare a mixed solution III.

[0057] 2) Add 4 mol of dopamine hydrochloride and 0.2 mol of acrylonitrile to the mixed solution III, and stir at a speed of 200 r / min for 13 minutes to prepare a modified solution for later use;

[0058] Step 3: Prepare alkaline modified solution:

[0059] 1) Dissolve 2.2 mol of Tris in 80 mL of deionized water and stir magnetically until the Tris is completely dissolved to prepare a Tris mixture;

[0060] 2) adding a tris(hydroxymethyl)aminomethane (Tris) mixed solution to the modified solution to obtain a mixed solution II;

[0061] 3) The pH value of the mixed solution II is then adjusted to 8.5 to obtain an alkaline modified solution;

[0062] Step 4: Prepare a reduced graphene oxide solution: Take 80 mL of graphene oxide dispersion and 80 mL of alkaline modified solution, slowly pour the alkaline modified solution into the graphene oxide dispersion, and incubate in a water bath at 50° C. for 22 hours to prepare a reduced graphene oxide solution;

[0063] Step 5: Prepare a silica gel mixture: Take 8 g of waste wind turbine blade powder and 80 mg of spherical silica powder, add the wind turbine blade powder and spherical silica powder to 150 mL of deionized water, and stir at a speed of 200 r / min for 90 minutes to prepare a silica gel mixture;

[0064] Step 6: Preparation of high-efficiency uranium adsorption composite gel material:

[0065] 1) adding 1.5 parts of the reduced graphene oxide solution to 2 parts of the silica gel mixture in a mass ratio, stirring at room temperature for 2 hours to prepare a mixture I;

[0066] 2) The mixed solution I is filtered to collect the product, which is then washed with deionized water until the pH value is neutral, and dried at 35° C. to obtain a high-efficiency uranium adsorption composite gel material.

[0067] Example 3 A high-efficiency uranium adsorption composite gel material and its preparation method

[0068] A highly efficient uranium adsorption composite gel material consists of a reduced graphene oxide solution and a silica gel mixture, wherein the silica gel mixture mainly consists of waste wind turbine blade powder and spherical silica powder.

[0069] The specific steps are as follows:

[0070] Step 1: Preparation of waste wind turbine blade powder:

[0071] Taking discarded wind turbine blades, cutting, crushing, pulverizing, grinding, and screening the discarded wind turbine blades to obtain discarded wind turbine blade powder, wherein the particle size of the discarded wind turbine blade powder is about 100 nm and is set aside;

[0072] Step 2: Prepare the modified solution:

[0073] 1) Take 180 mL of deionized water and 250 mL of ethanol by volume, add the deionized water to the ethanol, and stir at 150 r / min for 15 minutes to prepare a mixed solution III;

[0074] 2) Add 4 mol of dopamine hydrochloride and 1 mol of acrylonitrile to the mixed solution III, and stir at a speed of 150 r / min for 15 minutes to prepare a modified solution for later use;

[0075] Step 3: Prepare alkaline modified solution:

[0076] 1) Dissolve 2.8 mol of Tris in 150 mL of deionized water and stir magnetically until the Tris is completely dissolved to prepare a Tris mixture;

[0077] 2) adding a tris(hydroxymethyl)aminomethane (Tris) mixed solution to the modified solution to obtain a mixed solution II;

[0078] 3) The pH value of the mixed solution II is then adjusted to 8.5 to obtain an alkaline modified solution;

[0079] Step 4: Prepare a reduced graphene oxide solution: Take 150 mL of graphene oxide dispersion and 150 mL of alkaline modified solution, slowly pour the alkaline modified solution into the graphene oxide dispersion, and incubate in a water bath at 70° C. for 26 hours to prepare a reduced graphene oxide solution;

[0080] Step 5: Prepare a silica gel mixture: Take 15 g of waste wind turbine blade powder and 150 mg of spherical silica powder, add the wind turbine blade powder and spherical silica powder to 250 mL of deionized water, and stir at a speed of 150 r / min for 150 minutes to prepare a silica gel mixture;

[0081] Step 6: Preparation of high-efficiency uranium adsorption composite gel material:

[0082] 1) adding 2 parts of the reduced graphene oxide solution to 4 parts of the silica gel mixture in a mass ratio, stirring at room temperature for 4 hours to prepare a mixture I;

[0083] 2) The mixed solution I is filtered to collect the product, which is washed with deionized water until the pH value is neutral, and dried at 45° C. to obtain a high-efficiency uranium adsorption composite gel material.

[0084] The high-efficiency uranium adsorption composite gel material prepared in the present invention was observed by SEM scanning electron microscope, as shown in FIG. Figure 1 The following are the microscopic morphology images of composite gel (a); GO (b); GO-composite gel (c); PDA and acrylonitrile modified GO-composite gel (d)], namely composite gel, graphene oxide (GO), graphene oxide (GO)-composite gel and PDA and acrylonitrile modified graphene-composite gel (i.e., composite gel material with high efficiency in adsorbing uranium). Figure 1 As can be seen from (a)-(d), the silicon-waste wind turbine blade powder gel is a cluster of particles with a large porosity, while the graphene oxide (GO) is a two-dimensional layered structure with wrinkles on the surface, but the surface is relatively smooth. Due to the π-π interaction between the sheets, the stacking effect of graphene oxide (GO) is more obvious, connecting into larger sheets. Before PDA and acrylonitrile treatment, the composite gel and the graphene oxide (GO)-composite gel retain their respective morphologies. After PDA (polymerized dopamine) and acrylonitrile treatment, as shown in Figure 2, the morphology of the composite gel and the graphene oxide (GO)-composite gel remains unchanged. Figure 1 As shown in (d), it can be seen that graphene oxide (GO) is covered by a PDA (polymerized dopamine) layer, and the surface has better adhesion, which makes the modified PDA and acrylonitrile-graphene oxide-composite gel (i.e., high-efficiency uranium adsorption composite gel material) more tightly combined, increasing the specific surface area of ​​the high-efficiency uranium adsorption composite gel material without destroying the layered structure of graphene oxide.

[0085] Table 1 EDS spectrum comparison of high-efficiency uranium adsorption composite gel materials

[0086] element Weight percentage Weight percentage CK 27.64 32.08 OK 20.87 26.09 NK 0.00 1.02 Si K 37.13 30.28 Na K 0.31 0.21 Al K 3.87 3.03 Ca K 10.18 7.29

[0087] Table 1 shows that the carbon content increased from 27.64% to 32.08%, the oxygen content increased from 20.87% to 26.089%, the nitrogen content increased from 0% to 1.02%, and the silicon content decreased from 37.13% to 30.28%. The contents of other elements, such as Na, Al, and Ca, also decreased. This indicates that a layer of material adhered to the surface of the PDA-acrylonitrile-modified graphene-composite gel (i.e., the highly efficient uranium adsorption composite gel material).

[0088] The composite gel, graphene oxide, graphene oxide-composite gel and PDA and acrylonitrile modified graphene-composite gel were tested by infrared spectrometer. Figure 2 shown.

[0089] from Figure 2From the black line, we can see that at 1041cm -1 The hydroxyl CO stretching vibration peak is at 1620 cm -1 The peaks are aromatic C=C stretching vibrations, 1730 cm -1 The peak of carboxyl C=O stretching vibration is at 3420 cm -1 The characteristic band of graphene oxide (GO) is clearly seen at -OH. This shows that graphene oxide (GO) carries a large number of oxygen-containing groups such as carboxyl and hydroxyl groups. Pure PDA (polymerized dopamine) is at 1500 cm -1 There are NH bending vibration peaks and aromatic C=C stretching vibration peaks near 1730cm. In addition, compared with the spectrum of graphene oxide (GO), under the reduction of DA (dopamine), graphene oxide (GO) has a peak at 1730cm -1 The C=O vibration peak of the carboxyl group at 1041 cm -1 There is a hydroxyl CO stretching vibration peak at 1620 cm -1 There are vibration absorption peaks at the C=C double bonds in the GO skeleton. These phenomena indicate that GO is reduced by DA (dopamine) and PDA (polymerized dopamine) is "adhered" to GO.

[0090] The infrared spectrum of the surface of the regenerated fiber after PDA (polymerized dopamine) modification was tested using an infrared spectrometer. Figure 2 Further analysis found that at 3465cm -1 The OH stretching vibration absorption peak is at 3400 cm -1 The stretching vibration peak of NH appears; 1728cm -1 、1605cm -1 、1509cm -1 、1456cm -1 The absorption peak at 1647 cm is the C=O stretching vibration peak. -1 The NH bending vibration peak appears at 1320 cm -1 The stretching vibration peak of CN appeared, and the infrared spectrum analysis and EDS results together showed that the surface of the composite gel was successfully modified with amino groups.

[0091] Polydopamine and acrylonitrile are copolymerized by Figure 2 As can be seen from the green line in the figure, PDA and acrylonitrile modified graphene-composite gel (composite gel material with high efficiency adsorption of uranium) 2300cm -1 The presence of a C≡N bending vibration peak, characteristic of α- and β-aromatic cyanide compounds, indicates that the composite gel and graphene oxide surfaces were successfully modified with carbonyl groups, indicating that both amine and carbonyl groups were modified on the composite gel surface.

[0092] The surface of discarded wind turbine blade powder is mostly C=O groups, mostly alkane structures. After dopamine polymerization, it is affected by alkanes, the conjugation effect is weakened, and the absorption peak moves to the area with large wavenumbers, causing the absorption peak to blue-shift and the peak wavenumber to increase.

[0093] like Figure 3 As can be seen, the adsorption capacity of PDA (polymerized dopamine) and acrylonitrile modified graphene-composite gel (i.e., efficient adsorption uranium composite gel material) reaches a maximum value. By PDA (polymerized dopamine) and acrylonitrile, graphene oxide-composite gel is modified and the specific surface area of ​​efficient adsorption uranium composite gel material is increased. This is because the adding of graphene oxide (GO) has increased the specific surface area of ​​efficient adsorption uranium composite gel material, and more oxygen-containing groups (hydroxyl, carboxyl, amino etc.) are provided, so that the adsorption capacity of the efficient adsorption uranium composite gel material prepared by the present invention is enhanced. The adsorption capacity of the composite gel before unmodified can reach about 654ppm, but the adsorption capacity of the efficient adsorption uranium composite gel material prepared by the present invention far exceeds the adsorption capacity before modification, and the maximum adsorption capacity approximately reaches 864ppm.

[0094] The raw materials listed in the present invention, as well as the upper and lower limits and interval values ​​of the raw materials, and the upper and lower limits and interval values ​​of the process parameters can all realize the present invention, and the embodiments are not listed one by one here.

[0095] The above description is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principles of the present invention. These improvements and changes are also considered to be within the scope of protection of the present invention.

Claims

1. A highly efficient uranium adsorption composite gel material, characterized in that: The high-efficiency uranium adsorption composite gel material is composed of a reduced graphene oxide solution and a silica gel mixed solution; The silica gel mixture is mainly composed of waste wind turbine blade powder and spherical silica powder; The preparation method of the reduced graphene oxide solution is as follows: 80 mL to 150 mL of graphene oxide dispersion and 80 mL to 150 mL of alkaline modified solution are taken, the alkaline modified solution is slowly poured into the graphene oxide dispersion, and the reduced graphene oxide solution is prepared by water bathing at 50° C. to 70° C. for 22 to 26 hours; The preparation method of the alkaline modified solution is: 1) Dissolve 2.2 mol-2.8 mol of Tris in 80 mL-150 mL of deionized water, and stir magnetically until Tris is completely dissolved to obtain a Tris mixed solution; 2) Adding a mixture of tris(hydroxymethyl)aminomethane (Tris) into the modified solution to obtain a mixture II; 3) Then the pH value of the mixed solution II is adjusted to 8.5 to obtain an alkaline modified solution; The preparation method of the modified solution is: 1) Take 130mL-180mL of deionized water and 170mL-250mL of ethanol by volume, add the deionized water to the ethanol, stir for 10-15 minutes at a speed of 150-300r / min, and prepare a mixed solution III; 2) Add 1.5mol-4mol of dopamine hydrochloride and 0.2mol-1mol of acrylonitrile to the mixed solution III, stir for 10-15 minutes at a speed of 150-300r / min, and prepare a modified solution.

2. The method for preparing a highly efficient uranium adsorption composite gel material according to claim 1, characterized in that: The preparation method of the highly efficient uranium adsorption composite gel material comprises the following steps: 1) Preparation of silica gel mixture: 8g-15g of waste wind turbine blade powder and 80mg-150mg of spherical silicon powder are taken, the wind turbine blade powder and the spherical silicon powder are mixed, and then added into 150mL-250mL of deionized water, and stirred for 90-150 minutes at a speed of 150-300r / min to obtain silica gel mixture for standby use; 2) taking 1-2 parts of the reduced graphene oxide solution and 2-4 parts of the silica gel mixed solution by mass ratio, adding the reduced graphene oxide solution to the silica gel mixed solution, stirring at room temperature for 2-4 hours, to obtain a mixed solution I; 3) Filter the mixed solution I, collect the product, wash the product with deionized water until the pH value is neutral, and dry it at 35-45° C. to obtain a high-efficiency uranium adsorption composite gel material.

3. The method for preparing a highly efficient uranium adsorption composite gel material according to claim 2, characterized in that: The preparation method of the waste wind turbine blade powder is as follows: waste wind turbine blades are taken, and the waste wind turbine blades are cut, crushed, pulverized, ground and sieved to obtain the waste wind turbine blade powder.

4. The method for preparing a highly efficient uranium adsorption composite gel material according to claim 3, characterized in that: The particle size of the waste wind turbine blade powder is about 25 to 100 nm.