Silicon dioxide particles and preparation method thereof, and oral cleaning and care composition

By physically sealing the use of silica particles of specific particle size and density in dental care, the durability and safety of dentin allergies are solved, and the effect of rapid relief of tooth sensitivity and strong cleaning is achieved.

CN118164493BActive Publication Date: 2024-11-05ZHAOQING SANJIANG SILICON MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410228184.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-11-05
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

The prior art has short-lasting effects, safety risks and risks to special populations in alleviating dentin allergies, and traditional methods require long-term use or rely on chemical reactions.

Method used

Using silica particles with specific particle size and apparent density, the dentin tubes are physically sealed. The preparation method includes multiple reactions to control pH and temperature to form high-density and uniform silica particles for oral cleaning and care. Composition.

Benefits of technology

It achieves rapid, lasting and safe relief of tooth sensitivity, avoids the potential risks of chemical reactions, and provides the dual effects of strong cleaning and whitening of teeth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118164493B_ABST
    Figure CN118164493B_ABST
Patent Text Reader

Abstract

The present invention discloses a silicon dioxide particle and a preparation method thereof, and an oral cleaning and care composition. The silicon dioxide particle of the present invention satisfies the particle size: (D 90 ‑D 10 ) / D 50 =1.25~2.5,D 10 <1μm, D 30 =1.5μm~2μm, D 50 =3μm~4μm, D 75 <5.5μm, D 90 =6μm~8.5μm, D 97 <9μm, apparent density>0.3g / mL. The silica particles of the present invention have a small particle size, can effectively block the dentinal tubules and the micro-ducts on the surface of the teeth, isolate the channels of external stimuli, and hinder the conduction of excitement to the dental pulp nerves, thereby alleviating tooth sensitivity, and will not cause secondary damage to sensitive teeth without chemical reactions. It is safe and effective, with a long-lasting effect, and is suitable for preparing oral care compositions such as toothpaste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of oral care, and in particular to silicon dioxide particles and a preparation method thereof, and an oral cleaning and care composition. Background Art

[0002] Dentin hypersensitivity, also known as tooth hyperesthesia, is a symptom of pain caused by external stimuli such as temperature (cold, hot), chemical substances (acid, sweet), and mechanical action (friction, biting hard objects). It is characterized by rapid onset, sharp pain, and short duration. It is a relatively common oral problem. At present, there are two means to combat dentin sensitivity: 1) Remineralization through strontium salts and fluorides to block exposed dentinal tubules and reduce hydraulic conduction, isolate the channels connected to external stimuli, thereby achieving the effect of relieving and preventing tooth sensitivity. This method involves chemical reactions (for example, strontium salts enter the dentinal tubules and react with calcium in the tooth body to form calcified strontium apatite), which takes a relatively long time to really work, and chemical reactions in the mouth have unknown risks for special populations such as pregnant women and children; 2) Potassium salts, Chinese herbal medicines (for example, peony phenol), etc., play an analgesic role and paralyze the dental nerves to relieve tooth sensitivity, but it needs to be used for a long time. Once discontinued, the problem of tooth sensitivity may reappear.

[0003] Therefore, it is of great significance to develop an oral care product that can effectively alleviate tooth sensitivity, has a long-lasting effect, and is safe and environmentally friendly. Summary of the invention

[0004] The object of the present invention is to provide a silicon dioxide particle and a preparation method thereof, and an oral cleaning and care composition.

[0005] The technical solution adopted by the present invention is:

[0006] A silicon dioxide particle having a particle size (D 90 -D 10 ) / D 50 =1.25~2.5,D 10 <1μm, D 30 =1.5μm~2μm, D 50 =3μm~4μm, D 75 <5.5μm, D 90 =6μm~8.5μm, D 97 <9μm, apparent density>0.3g / mL.

[0007] Preferably, the particle size D of the silicon dioxide particles is 10 >0.5μm.

[0008] More preferably, the particle size D of the silicon dioxide particles is10 >0.7μm.

[0009] Preferably, the apparent density of the silica particles is >0.4 g / mL. High-density silica particles can be deposited more quickly into the exposed dentinal tubules during brushing, and are not easily shed during brushing, resulting in a more lasting effect.

[0010] Preferably, the copper consumption of the silicon dioxide particles is 2 mg to 11 mg, RDA is less than 140, and PCR is greater than or equal to 100. The copper consumption and RDA are small, the wear and tear on the teeth is small, the PCR is large, and the cleaning ability is strong.

[0011] Further preferably, the copper consumption of the silica particles is 4 mg to 7 mg, RDA is less than 135, and PCR is greater than or equal to 100.

[0012] Preferably, the water absorption of the silicon dioxide particles is less than 20 mL / 20 g.

[0013] More preferably, the water absorption of the silicon dioxide particles is less than 15 mL / 20 g.

[0014] Preferably, the dry agent ignition loss of the silicon dioxide particles is less than 8.5%.

[0015] More preferably, the dry agent ignition loss of the silicon dioxide particles is less than 6.5%.

[0016] Preferably, the silica particles are irregularly shaped.

[0017] A method for preparing the silicon dioxide particles as described above comprises the following steps:

[0018] 1) Dissolve polyethylene glycol in water, add sodium silicate solution and sulfuric acid solution at a certain flow rate, and control the pH value of the reaction solution to 1-2 during the reaction. The amount of sodium silicate solution added reaches 10m 3 ~15m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 2 to 4, and the reaction solution is aged to obtain an acidic silica sol;

[0019] 2) Add the acidic silica sol to the reaction tank, add a certain amount of sodium sulfate solution, heat to 50°C to 60°C and start stirring, add the sodium silicate solution and sulfuric acid solution at a certain flow rate, and control the pH value of the reaction solution to 7-9 and the temperature to 50°C to 60°C during the reaction, and react for 20min to 40min;

[0020] 3) Stop adding the sodium silicate solution and the sulfuric acid solution, raise the temperature to 60° C. to 70° C., add a certain amount of the sodium silicate solution, and add the sulfuric acid solution at a certain flow rate until the pH value of the reaction solution is 5 to 7, stop adding the sulfuric acid solution, and perform aging;

[0021] 4) Add a high concentration sulfuric acid solution at a constant flow rate until the pH value of the reaction solution is 3-5, stop adding the sulfuric acid solution, perform filter pressing, washing, drying and crushing to obtain silicon dioxide particles.

[0022] Preferably, the ratio of the polyethylene glycol to water in step 1) is 300kg to 400kg: 25m 3 ~35m 3 .

[0023] Preferably, the concentration of the sodium silicate solution in step 1) is 0.2 mol / L to 1 mol / L.

[0024] Preferably, the flow rate of the sodium silicate solution in step 1) is 1.5 m 3 / h~2.5m 3 / h.

[0025] Preferably, the concentration of the sulfuric acid solution in step 1) is 1 mol / L to 2 mol / L.

[0026] Preferably, the aging time in step 1) is 5 h to 7 h.

[0027] Preferably, the mass fraction of the acidic silica sol in step 2) is 1% to 3%.

[0028] Preferably, the mass fraction of the sodium sulfate solution in step 2) is 15% to 20%.

[0029] Preferably, the concentration of the sodium silicate solution in step 2) is 0.5 mol / L to 1.25 mol / L.

[0030] Preferably, the flow rate of the sodium silicate solution in step 2) is 5 m 3 / h~12m 3 / h.

[0031] Preferably, the concentration of the sulfuric acid solution in step 2) is 2 mol / L to 6 mol / L.

[0032] Preferably, in step 2), the volume ratio of the acidic silica sol, the sodium sulfate solution and the sodium silicate solution is 1:10-30:10-30.

[0033] Preferably, the concentration of the sodium silicate solution in step 3) is 0.5 mol / L to 1.25 mol / L.

[0034] Preferably, the amount of sodium silicate solution added in step 3) is 8 m 3 ~12m 3 .

[0035] Preferably, the flow rate of the sulfuric acid solution in step 3) is 2 m 3 / h~8m 3 / h.

[0036] Preferably, the aging time in step 3) is 10 min to 45 min.

[0037] Preferably, the volume fraction of the high concentration sulfuric acid solution in step 4) is 75% to 85%.

[0038] Preferably, the flow rate of the high concentration sulfuric acid solution in step 4) is 1 m / s. 3 / h~4m 3 / h.

[0039] An oral cleaning and care composition comprises the silicon dioxide particles.

[0040] Preferably, the oral cleaning and care composition further comprises an orally acceptable auxiliary material.

[0041] Preferably, the orally acceptable auxiliary material is at least one of a humectant, a thickener, a surfactant, an abrasive, and a flavor.

[0042] Preferably, the pH value of the oral cleaning and care composition is 6-10.

[0043] Preferably, the oral cleaning and care composition is toothpaste.

[0044] The present invention adopts a two-step method to carry out the reaction. First, sodium silicate solution and sulfuric acid solution are added to the silica sol system at a certain speed. When silicon dioxide nuclei are generated, the reaction conditions are changed, the temperature is raised to 60°C to 70°C, and the reaction is carried out in an alkaline environment. After reaching the specified pH value, a high-concentration sulfuric acid solution is added to adjust the end point pH value, and finally silicon dioxide particles are obtained. The specific reaction mechanism is as follows:

[0045] In step 2), acidic silica sol and sodium sulfate solution are added to the reaction tank (silica sol as a seed can increase the generation rate of silicon dioxide), the acidic silica sol is evenly dispersed in the entire reaction system, and the silicon dioxide generated by the reaction of sodium silicate and sulfuric acid preferentially grows on the surface of the silica sol to form silicon dioxide with uniform particle size and dispersion; high-concentration sodium sulfate solution as an electrolyte can accelerate the growth rate of silicon dioxide to form high-density, dense and uniform silicon dioxide;

[0046] In step 3), a certain amount of sodium silicate solution is first added to the reaction tank, and after the addition of the sodium silicate solution is stopped, sulfuric acid solution is added at a certain speed until the pH value of the reaction solution is 5 to 7. This step is a reaction mode in which acid is added to sodium silicate, and the growth rate of silicon dioxide is increased while maintaining the dispersed state of silicon dioxide, so that silicon dioxide with uniform particle size can be obtained;

[0047] In step 4), a high concentration of sulfuric acid solution is added to the reaction tank to reduce the surface hydroxyl content of silica, further reduce the polymerization of silica, ensure the uniformity of silica particle size and particle dispersibility, and reduce the agglomeration of silica finished products during the toothpaste preparation process.

[0048] The beneficial effects of the present invention are as follows: the silica particles of the present invention have a small particle size, can effectively block the dentinal tubules and the micro-ducts on the surface of the teeth, isolate the channels of external stimuli, and hinder the conduction of excitement to the dental pulp nerves, thereby alleviating tooth sensitivity, and will not cause secondary damage to sensitive teeth without chemical reaction. It is safe and effective, with a long-lasting effect, and is suitable for preparing oral cleaning and care compositions such as toothpaste.

[0049] Specifically:

[0050] 1) The silicon dioxide particles of the present invention solve the problems of long remineralization time, slow onset of effect, and potential safety hazards for special groups of people existing in remineralization anti-allergic products such as strontium salts and fluorides. It relieves tooth sensitivity through complete physical blocking, has a fast effect, does not cause chemical reactions, and is highly efficient and stable;

[0051] 2) The silicon dioxide particles of the present invention solve the problems of potassium salts and Chinese herbal medicine ingredients that paralyze dental nerves and relieve sensitivity only by reducing pain, etc. The silicon dioxide particles of the present invention control the structural density of the product so that it is not easy to fall off in the dentinal tubules, and the effect is long-lasting, which can effectively relieve tooth sensitivity.

[0052] 3) The silica particles of the present invention have a large apparent density and can be quickly deposited during the toothbrushing process, directly plugging the exposed dental tubules, with obvious effects. In addition, the silica itself has stable chemical properties, is acid and salt resistant, and does not cause any harm to the human body when deposited in the teeth, so it is a very safe plugging material;

[0053] 4) The silica particles of the present invention are used in anti-sensitivity toothpaste, which can not only relieve tooth sensitivity but also provide a strong cleaning effect, and has the dual effects of whitening teeth and relieving tooth sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is the SEM image of the silicon dioxide particles in Example 1. DETAILED DESCRIPTION

[0055] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0056] Embodiment 1:

[0057] A silicon dioxide particle, the preparation method of which is as follows:

[0058] 1) Dissolve 350 kg of polyethylene glycol-400 in 30 ml 3 of water, maintaining a certain flow rate while adding a 0.5 mol / L sodium silicate solution and a 1.5 mol / L sulfuric acid solution. The flow rate of the sodium silicate solution is 2m 3 / h, and the pH value of the reaction liquid was controlled to be 1 during the reaction. When the amount of sodium silicate solution added reached 12m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 3, and the reaction solution is allowed to stand for 6 hours to obtain an acidic silica sol;

[0059] 2) Mix 200L of 2% acidic silica sol and 5m 3 A 20% sodium sulfate solution was added to the reaction tank, and the stirring was started after the temperature was raised to 50°C. The stirring speed was 3500r / min. A sodium silicate solution with a concentration of 0.75mol / L and a sulfuric acid solution with a concentration of 4mol / L were added at a certain flow rate. The flow rate of the sodium silicate solution was 10m 3 / h, and control the pH value of the reaction solution to 7-8, the temperature to 50℃-60℃ during the reaction, and react for 30min;

[0060] 3) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C, and add 10m 3 The concentration of sodium silicate solution is 0.75 mol / L, maintaining 3.6 m 3 / h, add 4 mol / L sulfuric acid solution until the pH value of the reaction solution is 6-7, stop adding sulfuric acid solution, and let it stand for 25 minutes;

[0061] 4) Maintain 2m 3 A sulfuric acid solution with a volume fraction of 80% is added at a flow rate of / h until the pH value of the reaction solution reaches 4, and the addition of the sulfuric acid solution is stopped. The silicon dioxide particles are obtained by filter pressing, washing, drying and crushing.

[0062] The scanning electron microscope (SEM) image of the silicon dioxide particles in this example is as follows: Figure 1 shown.

[0063] Depend on Figure 1 It can be seen that the silica particles are irregular in shape.

[0064] Embodiment 2:

[0065] A silicon dioxide particle, the preparation method of which is as follows:

[0066] 1) Dissolve 350 kg of polyethylene glycol-400 in 30 ml 3 of water, maintaining a certain flow rate while adding a 0.5 mol / L sodium silicate solution and a 1.5 mol / L sulfuric acid solution. The flow rate of the sodium silicate solution is 2m 3 / h, and the pH value of the reaction liquid was controlled to be 1 during the reaction. When the amount of sodium silicate solution added reached 12m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 3, and the reaction solution is allowed to stand for 6 hours to obtain an acidic silica sol;

[0067] 2) Mix 200L of 2% acidic silica sol and 5m 3 A sodium sulfate solution with a mass fraction of 18% was added to the reaction tank. After heating to 50°C, stirring was started. The stirring speed was 3500r / min. A sodium silicate solution with a concentration of 0.75mol / L and a sulfuric acid solution with a concentration of 4mol / L were added while maintaining a certain flow rate. The flow rate of the sodium silicate solution was 10m 3 / h, and control the pH value of the reaction solution to 7-8, the temperature to 50℃-60℃ during the reaction, and react for 30min;

[0068] 3) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C, and add 10m 3 The concentration of sodium silicate solution is 0.75 mol / L, maintaining 3.6 m 3 / h, add 4 mol / L sulfuric acid solution until the pH value of the reaction solution is 6-7, stop adding sulfuric acid solution, and let it stand for 25 minutes;

[0069] 4) Maintain 2m 3 A sulfuric acid solution with a volume fraction of 80% is added at a flow rate of / h until the pH value of the reaction solution reaches 4, and the addition of the sulfuric acid solution is stopped. The silicon dioxide particles are obtained by filter pressing, washing, drying and crushing.

[0070] After testing (same as Example 1), the silicon dioxide particles of this example are irregular in shape.

[0071] Embodiment 3:

[0072] A silicon dioxide particle, the preparation method of which is as follows:

[0073] 1) Dissolve 350 kg of polyethylene glycol-400 in 30 ml 3 of water, maintaining a certain flow rate while adding a 0.5 mol / L sodium silicate solution and a 1.5 mol / L sulfuric acid solution. The flow rate of the sodium silicate solution is 2m 3 / h, and the pH value of the reaction liquid was controlled to be 1 during the reaction. When the amount of sodium silicate solution added reached 12m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 3, and the reaction solution is allowed to stand for 6 hours to obtain an acidic silica sol;

[0074] 2) Mix 200L of 2% acidic silica sol and 5m 3 A 15% sodium sulfate solution was added to the reaction tank, and the stirring was started after the temperature was raised to 50°C. The stirring speed was 3500r / min. A sodium silicate solution with a concentration of 0.75mol / L and a sulfuric acid solution with a concentration of 4mol / L were added while maintaining a certain flow rate. The flow rate of the sodium silicate solution was 10m 3 / h, and control the pH value of the reaction solution to 8-9 and the temperature to 50°C-60°C during the reaction, and react for 30 minutes;

[0075] 3) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C, and add 10m 3 The concentration of sodium silicate solution is 0.75 mol / L, maintaining 3.6 m 3 / h, add 4 mol / L sulfuric acid solution until the pH value of the reaction solution is 6-7, stop adding sulfuric acid solution, and let it stand for 25 minutes;

[0076] 4) Maintain 2m 3 A sulfuric acid solution with a volume fraction of 80% is added at a flow rate of / h until the pH value of the reaction solution reaches 4, and the addition of the sulfuric acid solution is stopped. The silicon dioxide particles are obtained by filter pressing, washing, drying and crushing.

[0077] After testing (same as Example 1), the silicon dioxide particles of this example are irregular in shape.

[0078] Comparative Example 1:

[0079] A silicon dioxide particle, the preparation method of which is as follows:

[0080] 1) Dissolve 350 kg of polyethylene glycol-400 in 30 ml 3 of water, maintaining a certain flow rate while adding a 0.5 mol / L sodium silicate solution and a 1.5 mol / L sulfuric acid solution. The flow rate of the sodium silicate solution is 2m 3 / h, and the pH value of the reaction liquid was controlled to be 1 during the reaction. When the amount of sodium silicate solution added reached 12m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 3, and the reaction solution is allowed to stand for 6 hours to obtain an acidic silica sol;

[0081] 2) Mix 200L of 2% acidic silica sol and 5m3 A 1% sodium sulfate solution was added to the reaction tank, and the stirring was started after the temperature was raised to 50°C. The stirring speed was 3500r / min. A sodium silicate solution with a concentration of 0.75mol / L and a sulfuric acid solution with a concentration of 4mol / L were added at a certain flow rate. The flow rate of the sodium silicate solution was 10m 3 / h, and control the pH value of the reaction solution to 7-8, the temperature to 50℃-60℃ during the reaction, and react for 30min;

[0082] 3) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C, and add 10m 3 The concentration of sodium silicate solution is 0.75 mol / L, and the 3 / h, add 4 mol / L sulfuric acid solution until the pH value of the reaction solution is 6-7, stop adding sulfuric acid solution, and let it stand for 25 minutes;

[0083] 4) Raise the temperature to 85℃~100℃ and maintain for 2m 3 A sulfuric acid solution with a volume fraction of 80% is added at a flow rate of / h until the pH value of the reaction solution reaches 4, and the addition of the sulfuric acid solution is stopped. The silicon dioxide particles are obtained by filter pressing, washing, drying and crushing.

[0084] Comparative Example 2:

[0085] A silicon dioxide particle, the preparation method of which is as follows:

[0086] 1) Mix 200L of deionized water and 5ml 3 A 1% sodium sulfate solution was added to the reaction tank, and the stirring was started after the temperature was raised to 50°C. The stirring speed was controlled to 3500r / min. A sodium silicate solution with a concentration of 0.75mol / L and a sulfuric acid solution with a concentration of 4mol / L were added at a certain flow rate. The flow rate of the sodium silicate solution was 10m 3 / h, and control the pH value of the reaction solution to 7-8, the temperature to 50℃-60℃ during the reaction, and react for 30min;

[0087] 2) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C, and add 10m 3 The concentration of sodium silicate solution is 0.75 mol / L, and the 3 / h, add 4 mol / L sulfuric acid solution until the pH value of the reaction solution is 6-7, stop adding sulfuric acid solution, and let it stand for 25 minutes;

[0088] 3) Raise the temperature to 85℃~100℃ and keep it for 2m 3A sulfuric acid solution with a volume fraction of 80% is added at a flow rate of / h until the pH value of the reaction solution reaches 4, and the addition of the sulfuric acid solution is stopped. The silicon dioxide particles are obtained by filter pressing, washing, drying and crushing.

[0089] Performance Test:

[0090] 1) The physical and chemical indicators of the silicon dioxide particles of Examples 1 to 3 and Comparative Examples 1 to 2 are shown in the following table:

[0091] Table 1 Physical and chemical indicators of silica particles

[0092] Physical and chemical indicators Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Water absorption (mL / 20g) 10.4 10.8 11.3 15.0 14.7 <![CDATA[Particle size D 10 (μm)]]> 0.725 0.852 0.933 2.993 3.096 <![CDATA[Particle size D 30 (μm)]]> 1.550 1.787 1.873 6.998 9.220 <![CDATA[Particle size D 50 (μm)]]> 3.552 3.773 3.822 25.324 36.432 <![CDATA[Particle size D 75 (μm)]]> 5.111 5.308 5.485 45.330 55.330 <![CDATA[Particle size D 90 (μm)]]> 7.554 8.003 8.255 60.229 78.123 <![CDATA[Particle size D 97 (μm)]]> 8.683 8.893 8.991 80.223 110.223 Apparent density (g / mL) 0.47 0.46 0.45 0.40 0.51 Copper consumption (mg) 4.20 5.09 6.78 9.20 12.10 Dry agent ignition loss (%) 6.4 6.2 6.3 6.0 5.8 RDA 124 130 133 180 230 PCR 104 102 100 108 110 Blockage rate (%) 86.46 80.47 78.37 11.65 8.57

[0093] Note:

[0094] Water absorption: Tested in accordance with "QB / T 2346-2015 Silicon Dioxide for Toothpaste in Oral Care Products";

[0095] Particle size D 10 , D 30 , D 50 , D 75 , D 90 and D 97 : Tested with reference to "GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method";

[0096] Copper loss: The test was conducted according to the method of the paper "Study on the Copper Loss Value of Silica for Toothpaste". The test process: Wash the copper sheet with distilled water and dry it, weigh and record the weight of the copper sheet, and then gently place and fix the copper sheet in the slot of the material pool. Accurately disperse different types of silica particles in deionized water, stir evenly and pour into the material pool to immerse the copper sheet. After rubbing back and forth 10,000 times, wash the copper sheet and dry it, weigh the difference before and after the friction of the copper sheet, and get the copper loss;

[0097] Dry agent ignition weight loss: Tested with reference to "QB / T 2346-2015 Silicon dioxide for toothpaste for oral hygiene care products";

[0098] RDA: Tested in accordance with "ISO 11609:2017";

[0099] PCR: Tested in accordance with "T / COCIA 7-2020 Toothpaste Efficacy Evaluation Laboratory Evaluation Method for Removal of Exogenous Stains";

[0100] Sealing rate: Referring to the tooth sealing rate calculation method in the group standard "T / COCIA 22-2023", the amount of silica added to the slurry used is 15%.

[0101] From Table 1, we can see that:

[0102] a) Compared with Example 1, the concentration of the sodium sulfate solution was reduced in Example 2 and Example 3, the particle size of the generated silicon dioxide particles was larger, and the uniformity of the particle size was reduced;

[0103] b) Compared with Example 1 and Example 2, the process pH value in Example 3 is increased, the water absorption of the generated silica particles is greater, the apparent density is reduced, and the plugging rate is slightly worse;

[0104] c) Compared with Example 1, the post-acidification temperature in Comparative Example 1 was greatly increased, and the concentration of the sodium sulfate solution was reduced, so that the particles grew rapidly during the reaction and formed large agglomerated particles;

[0105] d) In Comparative Example 2, no silica sol was added, and dispersed silicon dioxide with uniform particle size was not formed at the beginning. The particle size of the generated silicon dioxide particles was large and uneven, and the friction force increased.

[0106] 2) The silicon dioxide particles of Examples 1 to 3 and Comparative Examples 1 to 2 were used as abrasives to prepare toothpaste (toothpaste formula: 55wt% sorbitol, 20.4wt% distilled water, 1wt% carboxymethyl cellulose, 5wt% thickening silicon dioxide, 15wt% silicon dioxide particles, 0.1wt% sodium benzoate, 0.2wt% sodium saccharin, 2wt% sodium lauryl sulfate, 1wt% flavor and 0.3wt% titanium dioxide), and then the toothpaste was tested for performance. The test results are shown in the following table:

[0107] Table 2 Performance test results of toothpaste made of silicon dioxide particles of Examples 1 to 3 and Comparative Examples 1 to 2

[0108] Performance Indicators Blockage rate (%) Copper consumption (mg) Example 1 87.91 4.5 Example 2 83.45 5.4 Example 3 78.66 5.8 Comparative Example 1 30.20 8.4 Comparative Example 2 13.56 10.6

[0109] Note:

[0110] Occlusion rate: refer to the calculation method of tooth occlusion rate in the group standard "T / COCIA 22-2023";

[0111] Copper loss: The test process is similar to the copper loss test method of silica particles, and the test object is changed to toothpaste.

[0112] From Table 2, we can see that:

[0113] a) Compared with Example 1, the friction value of the silica particles in Examples 2 and 3 is larger, and the friction value of the toothpaste prepared is also larger. The particle size distribution can still achieve the function of blocking the dentinal tubules, and the blocking rate is lower than that of Example 1;

[0114] b) In Comparative Examples 1 and 2, the particle size of the silicon dioxide particles is too large, the toothpaste prepared has poor sealing effect and a high friction value.

[0115] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing silicon dioxide particles, characterized in that: The following steps are involved: 1) Dissolve polyethylene glycol in water, add sodium silicate solution and sulfuric acid solution at a certain flow rate, and control the pH value of the reaction solution to 1-2 during the reaction. The amount of sodium silicate solution added should reach 10m 3 ~15m 3 When the sulfuric acid solution is stopped, the sodium silicate solution is continued to be added until the pH value of the reaction solution reaches 2 to 4, and the reaction solution is aged to obtain an acidic silica sol; 2) Add acidic silica sol to the reaction tank, add a certain amount of sodium sulfate solution, heat it to 50℃~60℃ and start stirring, add sodium silicate solution and sulfuric acid solution at a certain flow rate, and control the pH value of the reaction liquid to 7~9 and the temperature to 50℃~60℃ during the reaction, and react for 20min~40min; 3) Stop adding sodium silicate solution and sulfuric acid solution, raise the temperature to 60°C to 70°C, add a certain amount of sodium silicate solution, maintain a certain flow rate and add sulfuric acid solution until the pH value of the reaction solution is 5 to 7, stop adding sulfuric acid solution, and carry out aging; 4) Add a high concentration of sulfuric acid solution at a constant flow rate until the pH value of the reaction solution is 3-5, stop adding the sulfuric acid solution, perform filter pressing, washing, drying and crushing to obtain silicon dioxide particles; Step 2) The mass fraction of the sodium sulfate solution is 15% to 20%; The particle size and apparent density of the silicon dioxide particles are as follows: 90 -D 10 ) / D 50 =1.25~2.5,D 10 <1μm, D 30 =1.5μm~2μm, D 50 =3μm~4μm, D 75 <5.5μm, D 90 =6μm~8.5μm, D 97 <9μm, apparent density>0.3g / mL.

2. The method for preparing silicon dioxide particles according to claim 1, characterized in that: The particle size D of the silica particles 10 >0.5μm.

3. The method for preparing silicon dioxide particles according to claim 1, characterized in that: The apparent density of the silica particles is >0.4 g / mL.

4. The method for preparing silicon dioxide particles according to any one of claims 1 to 3, characterized in that: The copper consumption of the silicon dioxide particles is 2 mg to 11 mg, RDA is less than 140, and PCR is greater than or equal to 100.

5. The method for preparing silicon dioxide particles according to any one of claims 1 to 3, characterized in that: The water absorption of the silicon dioxide particles is less than 20 mL / 20 g.

6. The method for preparing silicon dioxide particles according to any one of claims 1 to 3, characterized in that: The dry agent ignition loss of the silicon dioxide particles is less than 8.5%.