Long-life anti-halation glass and its preparation method and application
By optimizing the composition ratio and process processing of the glass composition, the problems of short service life of anti-halo glass and heavy metal pollution are solved, and a long-life anti-halo glass with high light transmittance and low cathode decay rate are achieved, suitable for intelligent vision and the field of photoelectric information processing.
Patent Information
- Application Number
- CN202410409303.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-07
AI Technical Summary
While providing light-transmitting performance, existing anti-halo glasses have problems with short service life and heavy metal pollution, which affect the performance and reliability of night vision systems.
The glass composition with SiO2, B2O3, Bi2O3, CaO, BaO, Al2O3, MgO, ZnO and CeO2 was prepared by adjusting the component ratio and process treatment. glass material.
It achieves a long-life anti-halo glass, with high transmittance, low cathode decay rate and chemical stability, avoids heavy metal pollution, and is suitable for intelligent vision technology and photoelectric information processing.
Smart Images

Figure CN118184137B_ABST
Abstract
Description
Technical Field
[0001] This application relates to special glass materials, and in particular to long-life anti-halo glass, its preparation method, and its application. Background Technology
[0002] Any discussion of prior art throughout the specification should not be construed as an admission that such prior art is well-known or constitutes part of common general knowledge in the art.
[0003] With the rapid development of technology, low-light night vision technology has become an important component in many fields, including military, security monitoring, and search and rescue. Especially in the day and night surveillance of the armed police and border defense forces, as well as in urban surveillance systems and search and rescue operations in underground mines, low-light night vision equipment plays a crucial role. Furthermore, its application in high-end fields such as high-performance cameras and spatial vision imaging detection systems is also increasing, demonstrating its wide range of uses and importance in modern technology. To meet the specific needs of these applications, higher standards have been set for the performance of key materials used in low-light night vision equipment, especially anti-halo glass.
[0004] Anti-halo glass plays a crucial role as a key material in second-generation and third-generation low-light night vision devices. Its main characteristic is high light transmittance across the ultraviolet, visible, and near-infrared spectral ranges, effectively improving the imaging quality of night vision devices. However, traditional anti-halo glass faces numerous technical challenges while providing the necessary light transmittance. For example, to achieve the anti-halo effect, a specific anti-halo coating is usually applied to the glass surface. This process not only reduces the glass's transmittance but may also shorten the product's lifespan due to weak adhesion between the coating and the glass.
[0005] More seriously, existing anti-halo glass often contains heavy metals such as As₂O₃, Sb₂O₃, and PbO. These substances have a significant negative impact on the cathode sensitivity of optical instruments, a phenomenon figuratively described as "poisoning." This "poisoning" effect severely affects the visible light transmittance and lifespan of the anti-halo glass, thereby impacting the performance and reliability of the entire night vision system. Summary of the Invention
[0006] Therefore, the purpose of this application is to provide a glass composition and a glass material prepared from the glass composition. The glass material can effectively prevent halo phenomenon, maintain high light transmittance, be free of heavy metal pollution, have good chemical stability and low cathode decay rate, and have a long service life. It can be widely used as an anti-halo glass material in the fields of intelligent vision technology or optoelectronic information processing technology.
[0007] Specifically, the present invention provides the following technical features, and the combination of one or more of the following technical features constitutes the technical solution of the present invention.
[0008] In a first aspect of the invention, a glass composition is provided, comprising or consisting of the following components in weight percentage: 40-60% SiO2, 10-30% B2O3, 3-5% Bi2O3, 3-5% CaO, 0.1-2% BaO, 0-3% Al2O3, 3-8% MgO, 0-4% ZnO, and 0-4% CeO2.
[0009] The selection of components and the interaction and balance between them in the glass composition described in this invention are crucial. The combination and effect of these components result in glass with the composition of this invention exhibiting excellent anti-halo effects, including better light transmittance, lower cathode fading rate, better resistance to crystallization, thus better chemical stability and a longer service life. In this invention, by carefully introducing and adjusting the contents of SiO2, B2O3, BaO, and CeO2, glass with uniform internal quality and stable composition can be prepared, exhibiting excellent transmittance and chemical stability. Simultaneously, by introducing and controlling the content of Bi2O3, the glass's ability to eliminate stray light is improved. Furthermore, the introduction and adjustment of the contents of Al2O3, MgO, ZnO, CaO, and B2O3 not only reduce the viscosity of the molten glass and the difficulty of forming, but also accelerate the melting process, reduce the tendency to crystallize, improve the chemical stability and mechanical properties of the glass, and facilitate processing and manufacturing.
[0010] In this invention, SiO2 (silicon dioxide) is the main component of the glass-forming body, forming the basis of the glass framework. Its high content in the glass helps to reduce the coefficient of thermal expansion and improve the glass's thermal stability, chemical stability, and heat resistance. In embodiments of this invention, the SiO2 content, by mass percentage, is 40-60%. In some embodiments of this invention, the SiO2 content, by mass percentage, may also be selected from the following ranges or any combination of the following ranges, or any value within the following ranges: 40-55%, 40-58%, 40-60%, 55-58%, 55-60%, 58-60%, etc. In some preferred embodiments of this invention, the SiO2 content, by mass percentage, is 40-58%, preferably 55-58%.
[0011] In this invention, B2O3 (boron trioxide) is also a glass-forming oxide. It not only improves the thermal and chemical stability of glass but can also replace SiO2 in some aspects, enhancing the stability of the glass network. However, the B2O3 content cannot be too high; otherwise, it will not be able to form a complete tetrahedral BO4 structure and will exist as trigonal BO3, thereby disrupting the network continuity and reducing the chemical stability of the glass. In the embodiments of this invention, the B2O3 content, by mass percentage, is 10-30%. In some embodiments of the present invention, the content of B2O3, expressed as a mass percentage, may be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 10.0-14.0%, 10.0-24.6%, 10.0-27.0%, 10.0-30.0%, 14.0-24.6%, 14.0-27.0%, 14.0-30.0%, 24.6-27.0%, 24.6-30.0%, 27.0-30.0%, etc. In some preferred embodiments of the present invention, the content of B2O3, expressed as a mass percentage, is 10-27%, 20-30%, or 14.5-30%.
[0012] In some embodiments of the present invention, the content of SiO2 is not less than 1.3 times the content of B2O3, for example, the ratio of SiO2 to B2O3 is 1.33-6, preferably 1.33-4, more preferably 1.33-2.5 or 2.3-6.
[0013] In this invention, Bi₂O₃ (bismuth trioxide) is introduced as a regulating oxide, affecting the thickness of the reduced layer (black layer) and its anti-spot properties after glass reduction. Although Bi₂O₃ has a relatively small toxic effect on the photocathode, improper use can actually reduce the cathode sensitivity of the glass. In embodiments of this invention, the Bi₂O₃ content is 3-5% by mass percentage. In some embodiments of this invention, the Bi₂O₃ content, by mass percentage, may also be selected from the following ranges or any ranges thereof, or any value within the following ranges: 3.0-4.0%, 3.0-4.9%, 3.0-5.0%, 4.0-4.9%, 4.0-5.0%, 4.9-5.0%, etc. In some preferred embodiments of this invention, the Bi₂O₃ content, by mass percentage, is 3.5-5%, preferably 3.5-4.9% or 4-5%.
[0014] In some embodiments of the present invention, the content of SiO2 is not less than 8 times the content of Bi2O3, for example, the ratio of SiO2 to Bi2O3 is 8-20, preferably 8-15, more preferably 8-12 or 11-14.5.
[0015] In this invention, CaO (calcium oxide) and BaO (barium oxide) are oxides used as the outer body of the network structure. The CaO content should not be too high, otherwise it will reduce the glass's chemical resistance and increase its crystallization tendency. BaO provides free oxygen, promotes glass melting, and can increase transmittance when used appropriately, but excessive amounts reduce chemical stability. In embodiments of this invention, the CaO content is 3-5% by mass percentage. In some embodiments of this invention, the CaO content, by mass percentage, may also be selected from the following ranges or any combination of the following ranges, or any value within the following ranges: 3.0-4.8%, 3.0-5.0%, 4.8-5.0%, etc. In some preferred embodiments of this invention, the CaO content is 3-4.8% or 4.8-5% by mass percentage.
[0016] In embodiments of the present invention, the BaO content, by mass percentage, is 0.1-2%. In some embodiments of the present invention, the BaO content, by mass percentage, may also be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 0.1-0.6%, 0.1-1.2%, 0.1-1.5%, 0.1-2.0%, 0.6-1.2%, 0.6-1.5%, 0.6-2.0%, 1.2-1.5%, 1.2-2.0%, 1.5-2.0%, etc. In some preferred embodiments of the present invention, the BaO content, by mass percentage, is 0.1-1.5%, preferably 0.1-1.2% or 0.1-0.5%.
[0017] In this invention, Al₂O₃ (aluminum oxide) and MgO (magnesium oxide) are used as regulating oxides. Their addition reduces the glass's crystallization tendency and coefficient of thermal expansion, and improves its thermal stability, chemical stability, and mechanical strength. However, excessive Al₂O₃ content increases the viscosity of the melt, making melting and refining difficult, and increasing the tendency to crystallize. Similarly, excessive MgO content also negatively impacts glass properties, increasing the tendency to crystallize, requiring higher annealing temperatures, and increasing manufacturing costs. In embodiments of this invention, the Al₂O₃ content is 0-3% by mass. In some embodiments of the present invention, the content of Al2O3, expressed as a mass percentage, may be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 0-0.6%, 0-2.0%, 0-2.4%, 0-3.0%, 0.6-2.0%, 0.6-2.4%, 0.6-3.0%, 2.0-2.4%, 2.0-3.0%, 2.4-3.0%, 0, etc. In some preferred embodiments of the present invention, the content of Al2O3, expressed as a mass percentage, is 0.5-3% or 0-2%, preferably 2-3% or 0.5-2% or 0.
[0018] In embodiments of the present invention, the MgO content, by mass percentage, is 3-8%. In some embodiments of the present invention, the MgO content, by mass percentage, may also be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 3.0-6.0%, 3.0-7.0%, 3.0-8.0%, 6.0-7.0%, 6.0-8.0%, 7.0-8.0%, etc. In some preferred embodiments of the present invention, the MgO content, by mass percentage, is 3-6.5% or 7.5-8%.
[0019] In this invention, ZnO acts as a network intermediate in the glass structure. It can exist as a [ZnO6] octahedron as the network exterior, improving the alkali resistance of the glass, or as a [ZnO4] structure to form the glass network. Simultaneously, it can replace Al2O3, appropriately reducing the amount of coloring oxides introduced into the raw materials and improving the glass transmittance. However, the ZnO content cannot be too high, otherwise it will increase the glass's coefficient of thermal expansion and increase its tendency for phase separation. In the embodiments of this invention, the ZnO content, by mass percentage, is 0-4%. In some embodiments of the present invention, the ZnO content, expressed as a mass percentage, may be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 0-0.5%, 0-1.4%, 0-3.5%, 0-4.0%, 0.5-1.4%, 0.5-3.5%, 0.5-4.0%, 1.4-3.5%, 1.4-4.0%, 3.5-4.0%, 0, etc. In some preferred embodiments of the present invention, the ZnO content, expressed as a mass percentage, is 0-3.5% or 0.5-4%, preferably 0-1.5% or 0.5-3.5%.
[0020] In some embodiments of the present invention, the content of Al2O3 is not less than 0.4 times the content of ZnO.
[0021] In this invention, CeO2 (cerium oxide) can act as a clarifying agent, promoting the removal of bubbles in molten glass at high temperatures, improving clarity and transparency. It can also act as a variable-valence oxide, suppressing color centers and enhancing glass performance. In embodiments of this invention, the CeO2 content, by mass percentage, is 0-4%. In some embodiments of this invention, the CeO2 content, by mass percentage, can also be selected from the following ranges or any range of values within the following ranges, or any value within the following ranges: 0-0.9%, 0-1.9%, 0-3.0%, 0-4.0%, 0.9-1.9%, 0.9-3.0%, 0.9-4.0%, 1.9-3.0%, 1.9-4.0%, 3.0-4.0%, 0, etc. In some preferred embodiments of this invention, the CeO2 content, by mass percentage, is 0-3.5% or 0.5-4%, preferably 0-2% or 0.5-2%.
[0022] In some embodiments of the present invention, the glass prepared by the glass composition according to the present invention has an average optical transmittance of ≥85%, ≥86%, ≥89%, ≥90%, or even ≥93% in the 400-1000 nm range. For example, in some embodiments, the glass has an average optical transmittance of 85-93% in the 400-1000 nm range, more preferably 90-93%.
[0023] In some embodiments of the present invention, the average cathode sensitivity of the glass prepared by the glass composition according to the present invention can be ≥754 μA / lm, ≥760 μA / lm, 770 μA / lm, or ≥778 μA / lm. For example, in some embodiments, the average cathode sensitivity of the glass is 754-778 μA / lm, preferably 760-778 μA / lm, and more preferably 770-778 μA / lm.
[0024] In some embodiments of the present invention, the glass prepared according to the glass composition of the present invention has a cathode fading rate of ≤4.5%, further ≤4%, and even further ≤3%. For example, in some embodiments, the imprint fading rate of the glass is 3-4.5%, preferably 3-4%.
[0025] In some embodiments of the present invention, the glass prepared by the glass composition according to the present invention has a coefficient of thermal expansion of (87.4-92.6)×10⁻⁶ at 20°C-300°C. -7 / ℃.
[0026] In some embodiments of the present invention, the glass prepared by the glass composition according to the present invention has a reduced layer thickness as low as 492 μm after reduction, and can be ≤553 μm, ≤549 μm, or ≤534 μm. For example, in some embodiments, the reduced layer thickness can be 492-553 μm. A relatively higher absorption rate (lower transmittance) can be achieved through a relatively thinner reduced layer.
[0027] In some embodiments of the present invention, the glass prepared by the glass composition according to the present invention, after reduction, has a transmittance of the reduced layer in the 400-1000 nm range as low as 0.07%, and can be as low as ≤0.09%, ≤0.1%, ≤0.15%, ≤0.2%, or ≤0.3%. For example, in some embodiments, the transmittance of the obtained reduced layer in the 400-1000 nm range can be 0.07-0.3%, 0.07-0.2%, 0.07-0.15%, or 0.07-0.1%.
[0028] In a second aspect of the invention, a glass preform is provided, which is made of the glass composition described in the first aspect above.
[0029] In some embodiments of the present invention, the preparation method of the glass blank includes: mixing the raw materials and melting them at 1400-1480°C, stirring, clarifying, and molding at 1110-1150°C to obtain the glass blank.
[0030] In some embodiments of the present invention, the melting time is 5-20 hours.
[0031] In some embodiments of the present invention, the stirring speed is 20-50 r / min and the stirring time is 8-16 h.
[0032] In some embodiments of the present invention, the forming time is 5-30 minutes. Rapid glass forming prevents the generation of secondary bubbles and impurities.
[0033] In embodiments of the present invention, melting and stirring can improve the uniformity and clarity of the molten glass. Low clarity of the molten glass can lead to air bubbles in the formed glass, reducing its quality. When the uniformity of the molten glass is low, it is prone to stratification or clumping, making it difficult to melt, clarify, and homogenize the glass, and in severe cases, even causing streaks or stone defects.
[0034] The method for preparing the preform according to this invention possesses process stability. The glass material prepared using this method exhibits stable properties and will not experience significant fluctuations in glass performance due to increases or decreases in the process parameters within this range. Of course, it is understood that within this process range, higher temperatures can shorten the preparation process compared to lower temperatures. If it is necessary to minimize time and cost, those skilled in the art can select a relatively higher temperature within the temperature range disclosed in this invention. In a third aspect of this invention, a long-life anti-halo glass is provided, comprising an effective light-transmitting region, wherein the glass composition of the effective light-transmitting region is as described in the first aspect above, or is made from the glass preform described in the second aspect above.
[0035] In some embodiments of the present invention, the long-life anti-halo glass further includes a reduction layer, which is obtained by reducing the glass in the effective light-transmitting area.
[0036] In some embodiments of the present invention, the reduction layer is located on the glass surface of the effective light-transmitting area.
[0037] In some embodiments of the present invention, the reduction process is carried out in a reducing atmosphere (such as hydrogen), wherein the reduction temperature is 550-650°C, the reduction time is 13500-14500 min, and the reduction pressure is 0.01-0.5 MPa.
[0038] In some embodiments of the present invention, the thickness of the reduction layer can be as low as 492 μm, and can be ≤553 μm, ≤549 μm, or ≤534 μm. For example, in some embodiments, the thickness of the reduction layer can be 492-553 μm. The long-life anti-halo glass of the present invention can achieve a relatively higher absorptivity (lower transmittance) through a relatively thinner reduction layer.
[0039] In some embodiments of the present invention, the transmittance of the reduction layer in the 400-1000 nm range can be as low as 0.07%, or as low as ≤0.09%, ≤0.1%, ≤0.15%, ≤0.2%, or ≤0.3%. For example, in some embodiments, the transmittance of the reduction layer in the 400-1000 nm range can be 0.07-0.3%, 0.07-0.2%, 0.07-0.15%, or 0.07-0.1%.
[0040] In some embodiments of the present invention, the average optical transmittance of the effective light-transmitting region in the 400-1000nm range can be ≥85%, ≥86%, ≥89%, ≥90%, or even ≥93%. For example, in some embodiments, the average optical transmittance of the glass in the 400-1000nm range is 85-93%, more preferably 90-93%.
[0041] In some embodiments of the present invention, the average cathode sensitivity of the long-life anti-halo glass can be ≥754 μA / lm, ≥760 μA / lm, 770 μA / lm, or ≥778 μA / lm. For example, in some embodiments, the average cathode sensitivity of the glass is 754-778 μA / lm, preferably 760-778 μA / lm, and more preferably 770-778 μA / lm.
[0042] In some embodiments of the present invention, the cathode fading rate of the long-life anti-halo glass is ≤4.5%, further ≤4%, and even further ≤3%. For example, in some embodiments, the imprint fading rate of the glass is 3-4.5%, preferably 3-4%.
[0043] In some embodiments of the present invention, the coefficient of thermal expansion of the long-life anti-halo glass at 20℃-300℃ is (87.4-92.6)×10⁻⁶. -7 / ℃. In a fourth aspect of the invention, a method for preparing the long-life anti-halo glass described in the third aspect above is provided, comprising:
[0044] After the raw materials are mixed, they are melted at 1400-1480℃, stirred, clarified, and shaped at 1110-1150℃ to obtain glass blanks.
[0045] After annealing, the glass preform is machined and then subjected to reduction treatment.
[0046] After the reduction process, the glass can be surface treated to appropriately expose the effective light-transmitting area.
[0047] In an embodiment of the present invention, annealing is performed to eliminate internal stress in the glass to meet the requirements of subsequent machining, and the annealing temperature is 500-620°C.
[0048] In embodiments of the present invention, the machining mainly includes one or more conventional machining processes such as grinding, polishing, fine carving, chamfering, and cutting, aiming to obtain glass of a certain size, shape, and surface condition. Appropriate processing methods can be selected as needed. For example, in some embodiments of the present invention, stepped glass can be obtained by performing machining steps such as rounding, rolling, slicing, and stepping on the annealed glass blank.
[0049] In embodiments of the present invention, the surface treatment includes, but is not limited to, grinding, polishing, cutting, and polishing, to adjust the surface condition of the glass, such as flatness and smoothness. Appropriate treatment methods can be selected as needed. For example, in some embodiments of the present invention, the stepped glass obtained by machining is subjected to a reduction treatment to form a reduction layer on the surface of the stepped glass. Then, the reduction layer on the upper and lower surfaces of the stepped glass is ground off and polished, exposing the transparent glass portion (i.e., exposing the effective light-transmitting area of the glass), while retaining the reduction layer on the remaining surfaces (stepped surfaces), thus obtaining the stepped, long-life anti-halo glass.
[0050] In some embodiments of the present invention, the reduction process is carried out in a reducing atmosphere (such as hydrogen), wherein the reduction temperature is 550-650°C, the reduction time is 13500-14500 min, and the reduction pressure is 0.01-0.5 MPa.
[0051] In a fifth aspect of the invention, an optical element is provided, which is made of the glass composition described in the first aspect or the glass blank described in the second aspect, or comprises the long-life anti-halo glass described in the third aspect.
[0052] In some embodiments of the present invention, the optical element is an optical window. In particular, in some embodiments, the optical window may be a cathode glass window or an anti-halo photoelectric glass input window.
[0053] In a sixth aspect of the invention, the glass composition described in the first aspect or the glass blank described in the second aspect is provided for use in the field of intelligent vision technology or optoelectronic information processing technology, or the glass comprising the long-life anti-halo glass described in the third aspect.
[0054] The field of intelligent vision technology combines optical imaging, photoelectric detection, image processing, and artificial intelligence to achieve environmental perception, understanding, and interaction. This fusion of technologies enables devices to not only capture high-quality images but also analyze and process them using intelligent algorithms to provide richer and more accurate information. For example, in security monitoring, urban surveillance systems utilize high-definition cameras and intelligent image analysis technology for facial recognition and behavior analysis to automate public safety monitoring. Low-light night vision devices and high-performance cameras, through advanced image enhancement technologies and intelligent noise reduction algorithms, provide clear visual information even in extremely low-light conditions. Space vision imaging and detection systems intelligently process image data captured from space for use in geographic information systems, environmental monitoring, and interstellar exploration. Underground mine search and rescue equipment combines photoelectric detection technology and intelligent image analysis to help search teams quickly locate trapped personnel in complex underground environments. The development of intelligent vision technology, especially combined with advancements in artificial intelligence and machine learning, is continuously expanding its applications in a wide range of fields, including industrial automation, medical imaging, environmental monitoring, and consumer electronics, becoming an important direction in modern technological development. In the aforementioned fields, such as in some embodiments of the present invention, the application is as an optical window in fields such as low-light night vision devices, high-performance cameras, spatial vision imaging and detection systems, urban surveillance systems, underground mine search and rescue, and high-end personal equipment. For example, it is a key component of optical input windows, cathode glass windows, or optical lenses to reduce halos and stray light, improve light transmittance and image clarity, thereby ensuring that these devices can capture optimal visual information under low light conditions or when high image quality is required.
[0055] For example, in these applications, the main functions and roles of the anti-halo glass may include:
[0056] Improve image sharpness and contrast: By reducing halo effects caused by light scattering and reflection, ensure that the imaging system can obtain sharper, higher-contrast images.
[0057] Enhanced photoelectric conversion efficiency: For devices that need to convert light signals into electrical signals (such as photomultiplier tubes in low-light night vision devices), anti-halo glass can ensure that as much effective light as possible is captured and converted, improving the sensitivity and performance of the device.
[0058] Protecting optical and optoelectronic components: As the external interface of the device, anti-glare glass not only provides optical functions, but also helps protect internal optical and optoelectronic components from physical damage and environmental influences.
[0059] To meet specific environmental requirements: In some special environments (such as space vision imaging detection and underground mine search and rescue), anti-halo glass also needs to have specific physical and chemical stability to adapt to extreme temperature, pressure or corrosive environments.
[0060] Through these functions, anti-glare glass plays an irreplaceable role in these high-end applications and is a key material for ensuring equipment performance and image quality.
[0061] The various specific technical features described in all embodiments of the above aspects of the present invention can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0062] Unless otherwise specified, the numerical range described in this invention includes all values within this range, and also includes any range value composed of any two values within this range. For example, 0-3.5% includes all values between 0 and 3.5%, and also includes any number of values within this range (e.g., 0%, 0.1%, 2.9%) and the range values they may form (e.g., 0-0.1%, 0-2.9%, 0.1-2.9%). Different values of the same indicator appearing in all embodiments of this invention can be arbitrarily combined to form a range value.
[0063] The following beneficial effects can be achieved through one or more of the above-mentioned technical means:
[0064] This invention provides a glass composition, from which glass is prepared exhibits good transmittance, with an average optical transmittance of ≥85% in the 400-1000 nm range, and an optimal transmittance of ≥93%; it also has a suitable melting temperature (1400-1480℃) and a suitable coefficient of thermal expansion, with a coefficient of thermal expansion of (87.4-92.6)×10⁻⁶ in the 20℃-300℃ range. -7 The glass exhibits good anti-crystallization properties at a temperature of / ℃ and possesses excellent chemical stability. Furthermore, this invention provides a long-life anti-halo glass with good optical transmittance, good cathode sensitivity, and, most importantly, a very low cathode decay rate, ≤4% within 12 months. This improves upon the problems of low transmittance and short lifespan of existing anti-halo glasses over a wide wavelength range. Attached Figure Description
[0065] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. The embodiments of this application will be described in detail below with reference to the accompanying drawings, wherein:
[0066] Figure 1This is a graph showing the average transmittance of the glass product of the present invention and the comparative glass product in the range of 400-1000 nm.
[0067] Figure 2 This is a graph showing the change in photocathode sensitivity over time for the glass product of the present invention and the comparative glass product. Detailed Implementation
[0068] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the manufacturer.
[0069] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of skill in the art. All reagents and materials used in this application are readily available through conventional means, and unless otherwise specified, they are used in accordance with conventional methods in the art or as per the product instructions. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to the methods of this application. The preferred embodiments and materials described herein are for illustrative purposes only.
[0070] The performance parameters in the following embodiments were obtained by measuring them using the following method:
[0071] The coefficient of thermal expansion of glass samples was tested using a DIL 402 thermal expansion measuring instrument from Netzsch GmbH, Germany. Sample preparation involved polishing the glass sample into a cylindrical strip measuring Φ6×50mm, with both ends parallel. The heating rate was set to 5℃ / min, and the data acquisition period was 20ms. The data were plotted as a temperature versus linear expansion curve, and the glass transition temperature and softening temperature were obtained using the tangent method. (GB / T 7962.16~2010)
[0072] Transmittance was tested using a UV-Vis-IR spectrophotometer. Sample preparation: The sample should be larger than the effective aperture, 20 mm thick, and polished on both sides. During testing, parameters such as wavelength range and scan speed were input, and the sample transmittance was measured. (GB / T7962.12-2010)
[0073] The acid and alkali resistance properties of glass samples were tested according to GB / T 7962.14-2010 and GB / T 7962.21-2019. For the acid resistance test, the sample was machined into a 20×20×10mm shape, with one large surface polished to a surface roughness Ra=0.05. Solutions with pH=2.9, pH=4.6, and pH=6.0 were used as the test medium. After the polished glass sample surface was eroded by the test medium, the time it took for the glass surface to exhibit violet-blue interference, discoloration, or peeling under an incandescent lamp was observed. The acid resistance stability of colorless optical glass was classified in descending order based on the duration of this erosion. For the alkali resistance test, the glass sample was machined into a 30×30×2mm shape, with all surfaces polished to a surface roughness Ra=0.012. The polished sample was immersed in a 0.01mol / L sodium hydroxide test solution at 50℃ for a specified time. The mass loss of the sample was measured, and the erosion depth was calculated based on the glass density. Based on the time t required to reach an erosion depth of 0.1 μm 0.1 The changes on the surface of the tested sample after etching are used to determine the alkali resistance stability level of the tested glass. The thickness of the reduced layer of the glass sample is measured using a stereomicroscope. The reduced glass slide should not be rough, without edge collapse or deformation, and the thickness of the black layer should be 0.5-0.6 mm with a transmittance of less than 1%.
[0074] The photosensitiveness of the anti-halo photoelectric glass was tested according to GJB 7351-2011. The cathode attenuation rate was characterized by calculating the photosensitiveness before and after attenuation. The test was performed on a second-generation image intensifier tube. The second-generation image intensifier tube was subjected to a specified voltage. A tungsten filament lamp with a color temperature of 2856K±50K was used as the light source. The luminous flux was uniformly distributed parallel to the input optical axis within a specified area of the photocathode. When a neutral density filter was used, the spectral characteristics of the input light radiation should not be changed. The cathode current was measured at this time. After the light source was cut off, the cathode current was measured when there was no light radiation input to the photocathode. The photosensitiveness was calculated according to formula (1):
[0075] S=(I1-I2) / Φ (1)
[0076] In the formula:
[0077] S—Photosensitivity, μA / lm;
[0078] I1—Cathode current when there is light radiation input, which is the sum of the photocurrent caused by light radiation and I2, in μA;
[0079] I2—Cathode current when there is no light radiation input, which is the sum of photocathode dark current and internal and external leakage current, μA;
[0080] Φ — Input luminous flux, lm.
[0081] The decay rate of the cathode of the anti-halo photoelectric glass is calculated using formula (2):
[0082]
[0083] In the formula:
[0084] S1—Initial cathode photosensitiveness, μA / lm;
[0085] S2—Cathode light sensitivity after a period of use, μA / lm.
[0086] The present invention will be further described below with reference to the embodiments.
[0087] Example 1
[0088] The glass composition and physical properties of this embodiment are shown in Table 1.
[0089] The preparation method is as follows: using quartz sand, boric acid, kaolin, bismuth nitrate, zinc nitrate, magnesium nitrate, barium oxide, and calcium oxide as raw materials, adding clarifying agent CeO2, the weight of the clarifying agent accounting for 4.0% of the weight of the high transmittance long life anti-halo glass, after thorough mixing, melting at 1430℃ for 9 hours, mechanical stirring (25 r / min, 10 hours), assisted high-temperature clarification, and molding at 1120℃ by casting or pouring (forming time is 5 minutes) to obtain glass blank.
[0090] The glass blank is mechanically processed to obtain stepped glass, which is then subjected to reduction treatment in a hydrogen reducing atmosphere. The reduction temperature is 637℃, the reduction time is 14000 min, and the reduction pressure is 0.18 MPa. After reduction treatment, a reduction layer is formed on the glass surface. The upper and lower surfaces of the stepped glass with the reduction layer are ground and polished to remove the reduction layer, exposing the transparent glass portion, while retaining the reduction layer on the remaining surfaces, thus obtaining anti-halo glass.
[0091] Example 2
[0092] The glass composition and physical properties of this embodiment are shown in Table 1.
[0093] In the preparation method, the clarifying agent is CeO2, and the weight of the clarifying agent accounts for 0.9% of the weight of the high transmittance long life anti-halo glass; the melting temperature is 1450℃, the melting time is 15h; mechanical stirring (30r / min, 13h), the molding temperature is 1130℃, the molding time is 20min, and other preparation steps and parameters are the same as in Example 1.
[0094] Example 3
[0095] The composition and physical properties of the glass in this embodiment are shown in Table 1.
[0096] In the preparation method, the clarifying agent is CeO2, and the weight of the clarifying agent accounts for 1.9% of the weight of the high transmittance long life anti-halo glass; the melting temperature is 1440℃, the melting time is 18h; mechanical stirring (30r / min, 15h), the molding temperature is 1140℃, the molding time is 25min, and other preparation steps and parameters are the same as in Example 1.
[0097] Example 4
[0098] The composition and physical properties of the glass in this embodiment are shown in Table 1.
[0099] In the preparation method, the clarifying agent is CeO2, and the weight of the clarifying agent accounts for 3.0% of the weight of the high transmittance long life anti-halo glass; the melting temperature is 1440℃, the melting time is 11h; mechanical stirring (30r / min, 15h), the molding temperature is 1140℃, the molding time is 20min, and other preparation steps and parameters are the same as in Example 1.
[0100] Example 5
[0101] The composition and physical properties of the glass in this embodiment are shown in Table 1.
[0102] In the preparation method, the clarifying agent is CeO2, and the weight of the clarifying agent accounts for 4.0% of the weight of the high transmittance long life anti-halo glass; the melting temperature is 1480℃, the melting time is 18h; mechanical stirring (40r / min, 15h), the molding temperature is 1130℃, the molding time is 25min, and other preparation steps and parameters are the same as in Example 1.
[0103] Example 6
[0104] The composition and physical properties of the glass in this embodiment are shown in Table 1.
[0105] In the preparation method, no glass clarifying agent is added; the melting temperature is 1440℃ and the melting time is 15h; mechanical stirring (35r / min, 15h); the molding temperature is 1140℃ and the molding time is 25min; other preparation steps and parameters are the same as in Example 1.
[0106] Comparative Examples 1-4
[0107] The composition and physical properties of the glasses in Comparative Examples 1-4 are shown in Table 1.
[0108] The glass preparation methods in Comparative Examples 1-4 are the same as in Example 1.
[0109] Table 1. Composition, content, and physical properties of the glasses in Examples 1-6 and the comparative examples of the present invention.
[0110]
[0111]
[0112] The glass products of Examples 1-6 exhibit better optical transmittance and less "poisoning" effect on the cathode, thus improving the service life of the anti-halo glass. As shown in Table 1, the glass products prepared in Examples 1-6 of this invention have an average optical transmittance of ≥85% in the 400-1000nm range, a cathode sensitivity of ≥754μA / lm, and a cathode decay rate of less than 4.5%, while also possessing good chemical stability.
[0113] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A long-life anti-halation glass, comprising a light-transmitting effective area and a reduction layer, wherein the reduction layer is obtained by reducing the light-transmitting effective area glass, in, The light-transmitting effective area is composed of the following components in terms of mass percentage: SiO 2 40-60%, B 2 O 3 20-30%, Bi 2 O 3 3-5%, CaO 3-5%, BaO 0.1-2%, Al 2 O 3 0-3%, MgO 3-8%, ZnO 0-4% and CeO 2 0-4%.
2. The long-life anti-halation glass according to claim 1, It is characterized in that SiO 2 The content is not less than B 2 O 3 1.3 times the content.
3. The long-life anti-halation glass according to claim 1, It is characterized in that SiO 2 The content is not less than Bi 2 O 3 8 times the content.
4. The long-life anti-halation glass according to claim 1, It is characterized in that Al 2 O 3 The content of ZnO is not less than 0.4 times the content of ZnO.
5. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, SiO 2 The content is 40-58%.
6. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, SiO 2 The content is 55-58%.
7. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Bi 2 O 3 The content is 3.5-5%.
8. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Bi 2 O 3 The content is 4-5%.
9. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, the CaO content is 3-4.8%.
10. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, the CaO content is 4.8-5%.
11. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, the BaO content is 0.1-1.5%.
12. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the BaO content is 0.1-1.2%.
13. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of BaO is 0.1-0.5%.
14. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Al 2 O 3 The content is 0.5-3%.
15. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Al 2 O 3 The content is 0-2%.
16. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Al 2 O 3 The content is 2-3%.
17. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Al 2 O 3 The content is 0.5-2%.
18. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, Al 2 O 3 The content is 0.
19. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of MgO is 3-6.5%.
20. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of MgO is 7.5-8%.
21. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of ZnO is 0-3.5%.
22. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of ZnO is 0.5-4%.
23. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of ZnO is 0-1.5%.
24. The long-life anti-halation glass according to claim 1, It is characterized in that Calculated by mass percentage, the content of ZnO is 0.5-3.5%.
25. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, CeO 2 The content is 0-3.5%.
26. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, CeO 2 The content is 0.5-4%.
27. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, CeO 2 The content is 0-2%.
28. The long-life anti-halation glass according to claim 1, It is characterized in that In terms of mass percentage, CeO 2 The content is 0.5-2%.
29. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The reduction layer is located on the glass surface in the light transmission effective area.
30. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The reduction treatment is carried out in a reducing atmosphere, wherein the reduction temperature is 550-650° C., the reduction time is 13500-14500 min, and the reduction pressure is 0.01-0.5 MPa.
31. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The thickness of the reduction layer is 492-553 μm.
32. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The optical transmittance of the reducing layer at 400-1000 nm is 0.07-0.3%.
33. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The average optical transmittance of the light-transmitting effective area in the range of 400-1000 nm is ≥85%.
34. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The average cathode sensitivity of the long-life anti-halation glass is 754-778 μA / lm.
35. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The cathode decay rate of the long-life anti-halation glass is ≤4.5%.
36. The long-life anti-halation glass according to any one of claims 1 to 28, It is characterized in that The thermal expansion coefficient of the long-life anti-halation glass at 20°C-300°C is (87.4-92.6)×10 -7 / ℃.
37. A method for preparing the long-life anti-halation glass according to any one of claims 1 to 36, wherein include: After the raw materials are mixed, they are melted at 1400-1480°C, stirred, clarified, and molded at 1110-1150°C to obtain glass blanks; After the glass blank is annealed at 500-620°C, it is machined, and the obtained glass material is reduced to form a reduction layer on the surface of the glass material.
38. The method according to claim 37, It is characterized in that The reduction treatment is carried out in a reducing atmosphere, wherein the reduction temperature is 550-650° C., the reduction time is 13500-14500 min, and the reduction pressure is 0.01-0.5 MPa.
39. An optical element comprising the long-life anti-halation glass according to any one of claims 1 to 36.
40. The optical element according to claim 39, It is characterized in that The optical element is an optical window.
41. The optical element according to claim 40, It is characterized in that The optical window is a cathode glass window or an anti-halation photoelectric glass input window.
42. Use of the long-life anti-halation glass according to any one of claims 1 to 36 in the field of intelligent vision technology or optoelectronic information processing technology.
43. The use according to claim 42, It is characterized in that The applications include being used as optical windows in low-light-level night vision devices, high-performance cameras, space visual imaging detection systems, urban Skynet monitoring systems, and underground mine search and rescue.
44. The use according to claim 43, It is characterized in that The long-life anti-halation glass is used as a cathode glass window or an anti-halation photoelectric glass input window.
Citation Information
Patent Citations
Borosilicate glass, anti-halo input window glass and preparation method thereof
CN108423986A
Fire-polishing blackening preparation method of anti-halation step-like glass
CN109704555A
Glass article with blackened layer and method of making same
CN117088607A
Glass material, glass article having blackened layer, and method of making same
CN117088608A
UV-blocking borosilicate glass, the use of the same, and a fluorescent lamp
CN1653007A