A high-transparency adhesive tape and its preparation method and application

By using high-permeability tape in lithium batteries, combining porous substrates and olefin polymer adhesive layers, the problems of pole sheet cracking and lithium separation during hot pressing and circulation of lithium batteries are solved, and the safety of batteries is achieved Extended sex and life span.

CN118185490BActive Publication Date: 2024-11-12STEADYCHEM (SHANGHAI) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410301437.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-11-12
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

The existing lithium battery tape cannot effectively prevent the electrode sheet from cracking during hot pressing, and causes lithium electrode removal during battery circulation, affecting the safety and life of the battery.

Method used

Using high-permeability tape, including laminated porous substrate and adhesive layer, a discontinuous adhesive layer is formed by coating the thermoplastic coating liquid, and the use of olefin polymers to provide structural support and chemical stability while maintaining high Breathability and low cost.

Benefits of technology

Without affecting the transmission of lithium ions, the protection electrode sheet is not cracked, and the electrode is prevented from excision during the battery cycle, extending the battery life, and improving the battery safety and charging and discharging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118185490B_ABST
    Figure CN118185490B_ABST
Patent Text Reader

Abstract

The invention discloses a highly permeable tape and a preparation method and application thereof, wherein the tape comprises a laminated porous substrate and an adhesive layer; the porous substrate has a thickness of 5-50 μm and an air permeability of 50-450 s / 100 ml, and comprises at least one of a porous diaphragm and a non-woven fabric; the adhesive layer is formed by applying a thermoplastic coating liquid to at least one surface of the porous substrate to form a non-continuous adhesive layer; the thermoplastic coating liquid is an aqueous coating liquid or a solvent-based coating liquid, comprising an olefin polymer and an optional tackifying resin; the initial air permeability P1 of the tape is ≤2.5×P0, where P0 is the air permeability of the porous substrate; the air permeability P2 is ≤4.0×P1 after high temperature aging; and the air permeability P3 is ≤1.2×P1 after being soaked in electrolyte. The tape can protect the pole piece during hot pressing without affecting the passage of lithium ions, and can protect the electrode during battery cycling to prevent the battery from lithium precipitation, thereby extending the battery life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery tapes, and in particular relates to a high-transparency tape and a preparation method and application thereof. Background Art

[0002] In the normal production process of lithium batteries, the positive electrode sheets are wound with the separator and the negative electrode sheets, and then undergo processes such as hot pressing, liquid injection, and chemical formation to prepare the battery cells. Since the electrode sheets are somewhat brittle, the bending amplitude of the electrode sheets wound in the inner layer of the battery cells is often large at the corners of the battery cells, and there is a large stress, which leads to easy cracking after hot pressing, and the active material falls off, thus affecting the yield rate and safety of the battery cells, or causing lithium deposition at the corners during the battery cycle, and causing the wound battery cells to deform, so that the electrode sheets at the corners are at risk of breaking, affecting the safety performance and cycle performance of the battery.

[0003] Pasting tape on the pole piece at the corresponding position can effectively prevent the pole piece from hot pressing cracking, lithium deposition at the corner of the battery cell, deformation and fracture of the battery cell. Using flexible substrate tape can prevent the cracking of the tape substrate. The tape used in conventional lithium batteries is generally electrolyte-resistant, and the adhesive used in the glue layer is generally acrylic pressure-sensitive adhesive, hot melt adhesive, etc. The substrate is generally PET, BOPP film, etc. These types of tapes have low solubility in the electrolyte and are not permeable to lithium ions, which limits their use in the corners inside the battery cell.

[0004] Invention CN101017916A discloses a high-safety lithium-ion battery with a protective film attached to the diaphragm, including a positive electrode, a negative electrode, a diaphragm, an electrolyte and a battery shell. A tape or film is arranged at the edge of the diaphragm at the start and end of the electrode coating. The diaphragm with the tape or film is placed between the positive electrode and the negative electrode. The positive electrode, diaphragm and negative electrode are wound to form an electrode group, which is arranged in the battery shell, and then the liquid injection, sealing and chemical formation process are carried out to obtain a lithium-ion battery. The thickness of the tape or film on the diaphragm is 10μm to 30μm. The film adopts a spray-polymerized film or a hot-pressed acrylic PP film, and the film is polymerized by photopolymerization or thermal polymerization, and the temperature of the thermal polymerization is less than or equal to 90°C. However, the PP adhesive layer with a full coverage thickness of 10-30μm set in the invention greatly reduces the lithium ion permeability of the diaphragm, resulting in lithium ion accumulation at the electrode corners, causing lithium precipitation, and reducing battery performance.

[0005] Invention CN115651554A discloses a battery separator tape with a soluble adhesive layer and a preparation method thereof, comprising a battery separator and an adhesive layer arranged on the surface of the battery separator, wherein the adhesive forming the adhesive layer comprises the following raw materials in weight percentage: 40-60% solvent-based polyacrylate; 10-30% polyvinyl acetate; 5-15% polystyrene resin; 0.1-0.5% initiator; 0.5-1.0% curing agent; 0-30% solvent. The adhesive layer of the tape provided by the invention can be quickly dissolved in the electrolyte and will not block the normal migration of lithium ions. However, after the tape is dissolved, it cannot continue to provide support for the corners, resulting in rupture of the separator, which may cause a short circuit, and may also form an uneven electric field on the negative electrode surface, promoting the occurrence of lithium precipitation.

[0006] Therefore, how to optimize the existing electrolyte-resistant battery tape materials and structures so that the tape can protect the electrode from cracking under stress during the hot pressing process without affecting the passage of lithium ions, and can also protect the electrode diaphragm during the battery cycle to prevent lithium deposition in the battery, thereby extending the battery life is an urgent problem to be solved by technical personnel in this field. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a high-permeability tape and a preparation method and application thereof, which is particularly suitable for lithium batteries. Without affecting the passage of lithium ions, the high-permeability lithium battery tape can not only protect the electrode from cracking under stress during the hot pressing process, but also protect the electrode diaphragm to prevent lithium deposition in the battery during the battery cycle.

[0008] In a first aspect, the present invention provides a high-transparency adhesive tape, comprising a laminated porous substrate and an adhesive layer;

[0009] The porous substrate has a thickness of 5-50 μm and an air permeability of 50-450 s / 100 ml, and includes at least one of a porous membrane and a non-woven fabric;

[0010] The adhesive layer is formed by coating a thermoplastic coating liquid on at least one surface of the porous substrate to form a discontinuous adhesive layer; the thermoplastic coating liquid is an aqueous coating liquid or a solvent-based coating liquid, comprising an olefin polymer and an optional tackifying resin;

[0011] The initial air permeability of the tape is P1≤2.5×P0, where P0 is the air permeability of the porous substrate;

[0012] After high temperature aging, the air permeability of the tape is P2≤4×P1;

[0013] After soaking in electrolyte, the air permeability of the tape is P3≤1.2×P1.

[0014] The adhesive layer of the present invention is a discontinuous adhesive layer comprising an olefin polymer. Since the olefin polymer has excellent chemical stability and mechanical strength, it can provide good structural support for it during the battery operation process, and is not corroded by the electrolyte at the same time, and the olefin polymer cost is relatively low, which can reduce the overall cost of the battery, so the present invention uses an olefin polymer as the main material of the adhesive layer. But at the same time, the olefin polymer has a high-temperature self-closing property, which will automatically close the pores under high temperature conditions, resulting in a decrease in the permeability of the glue layer. In order to eliminate the impact of this characteristic in the adhesive layer, the present invention first uses olefin polymers to form an aqueous or solvent-based thermoplastic coating liquid, and then the coating liquid is arranged on a porous substrate with excellent permeability, and a discontinuous adhesive layer is obtained after drying, and the volume ratio of water or solvent in the coating liquid is used to increase the opening between the glue layers to increase the overall permeability of the tape while ensuring bonding performance and mechanical strength. Secondly, when the present invention uses an aqueous coating liquid, the microsphere-shaped olefin polymer in the aqueous emulsion can maintain its appearance shape under high temperature conditions and will not block the lithium ion transmission channel.

[0015] Preferably, after high-temperature aging of the tape (for example, after baking at 110°C for 24 hours, taking it out and cooling it to room temperature for testing), the air permeability of the tape is P2≤2.5×P1, and more preferably P2 satisfies: P2=A h ×P1-B h , where A h The value is 1.2-2.2, B h The value is 0-30; after soaking in electrolyte (for example, completely immersed in electrolyte solvent, baked at 85°C for 24 hours, taken out, wiped clean and left for 20 minutes before testing, the electrolyte solvent contains ethylene carbonate EC 20wt%, ethyl methyl carbonate EMC 50wt% and ethyl propionate EP 30wt%), the tape air permeability P3 satisfies: P3 = A e ×P1+B e , where A e The value is 1.02-1.1, B e The value range is 0-15.

[0016] Preferably, the olefin polymer has a melting point of 60-150° C. and is selected from at least one of polyolefin resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-methacrylic acid copolymers, and polyvinylidene fluoride;

[0017] The tackifying resin is selected from at least one of hydrogenated C5, hydrogenated C9 resin, hydrogenated C5 / C9 copolymer resin, hydrogenated DCPD, hydrogenated rosin, and hydrogenated polyterpene resin.

[0018] Preferably, the polyolefin resin is selected from at least one of polypropylene resin, amorphous α-olefin copolymer, ethylene-octene or ethylene-butene copolymer, maleic anhydride grafted polyolefin, acrylic acid grafted polyolefin, methacrylic acid grafted polyolefin, acrylic acid / methacrylic acid blended modified polyolefin.

[0019] Preferably, the porous substrate comprises a porous membrane with a porosity of 30-60%, selected from at least one of a single-layer PP membrane, a multi-layer PP membrane, a single-layer PE membrane, a multi-layer PE membrane, a PP / PE composite membrane, a PP / PE / PP sandwich membrane, and a PVDF membrane; and / or

[0020] The porous substrate comprises a non-woven fabric with a pore size of ≤10 μm, and is selected from at least one of PP non-woven fabric, PE non-woven fabric, PET non-woven fabric, and PTFE non-woven fabric.

[0021] The porous substrate used in the present invention has a higher porosity than solid film materials such as PET film, PI film, and BOPP film. These pores allow the electrolyte to penetrate more easily, thereby providing a better ion conduction path, which can reduce internal resistance and improve the power output of the battery. At the same time, the above-mentioned porous substrates, such as porous PP and PE materials, have a relatively high melting point at high temperatures, which helps to maintain the integrity of the diaphragm when the battery is overheated and reduce the risk of short circuits.

[0022] Preferably, the thermoplastic coating liquid is an aqueous coating liquid, and comprises the following raw materials in parts by weight:

[0023] 98-99.5 parts of aqueous emulsion;

[0024] Inorganic filler 0-40 parts;

[0025] Wetting agent 0-2 parts;

[0026] The solid content of the aqueous emulsion is 1-40%, and emulsion microspheres are dispersed therein, the emulsion microspheres contain the olefin polymer, and the particle size D50 of the emulsion microspheres is 0.2-2 μm;

[0027] The inorganic filler includes at least one of aluminum hydroxide, aluminum oxide, boehmite, zinc oxide, magnesium oxide, and boron nitride, and the particle size D50 is 0.5-5 μm;

[0028] The wetting agent includes an anionic wetting agent or a nonionic wetting agent. Specifically, the anionic wetting agent includes at least one of alkyl sulfate, alkyl sulfonate, higher fatty acid salt, phosphate ester salt, fatty acid or fatty acid sulfate ester salt; the nonionic wetting agent includes at least one of polyoxyethylene alkylphenol ether, polyoxyethylene fatty alcohol ether, and EO / PO block copolymer, and the HLB value is between 5-20, preferably 7-13.

[0029] The aqueous coating liquid used in the present invention can form a uniform but discontinuous adhesive layer on the surface of the tape using the emulsion microsphere drying technology. This uniformity helps to ensure the uniform distribution of the electrolyte and the ion transmission, thereby improving the overall performance and stability of the battery. At the same time, by adjusting the composition, size and concentration of the emulsion microspheres, the microstructure of the adhesive layer, including the porosity and pore size distribution, can be precisely controlled. This control can optimize the permeability of the electrolyte and the transmission speed of the ions, which is crucial to improving the charge and discharge efficiency and power density of the battery. And by adding different functional materials to the emulsion, such as conductive materials, flame retardants or self-healing materials, additional functions can be given to the tape without sacrificing air permeability and moisture permeability. This versatility makes the battery design more flexible and can meet specific application requirements.

[0030] Preferably, the aqueous emulsion further comprises 0.01-10wt% of an emulsifier, and optionally an auxiliary emulsifier and a defoaming agent;

[0031] The emulsifier is selected from at least one of C8-C18 higher fatty acid salts, alkyl sulfates, alkyl sulfonates, phosphate esters, polyoxyethylene fatty alcohol ethers, polyoxyethylene alkylphenol ethers with EO segments ≤ 20, and EO / PO block copolymers with EO+PO segments of 20-80;

[0032] The auxiliary emulsifier is selected from C2-C5 short-chain alcohols or polyglycerol esters. The auxiliary emulsifier is evaporated when the aqueous emulsion is prepared, and there is basically no residue in the aqueous coating liquid and the final adhesive layer.

[0033] The defoaming agent is selected from one or more of polysiloxane defoaming agents, silicone emulsion defoaming agents, polyether defoaming agents, polyether modified silicon defoaming agents, and higher alcohol defoaming agents.

[0034] The preparation of the aqueous coating liquid can be prepared according to the above-mentioned raw material ratio and with reference to the existing emulsion preparation technology. Among them, the aqueous emulsion dispersed with emulsion microspheres can be prepared by hot melt method, granulation dispersion method, phase inversion method and other processes. The particle size of the emulsion microspheres can be controlled by controlling the type and amount parameters of the emulsifier, co-emulsifier, solvent, etc., as well as the process parameters such as heating temperature, high-speed dispersion / shear rate, pressure, time, etc. After that, inorganic fillers, color powder, wetting agent and other components are matched as needed to prepare the aqueous coating liquid.

[0035] Preferably, the thermoplastic coating liquid is a solvent-based coating liquid, comprising the olefin polymer and a solvent and an optional inorganic filler, the concentration of the olefin polymer is 5-20wt%, and the solvent-based coating liquid forms the discontinuous bonding layer by spraying. Wherein, the solvent is selected from at least one of an aromatic hydrocarbon solvent, a ketone solvent, and an aliphatic hydrocarbon solvent. The mass concentration of the inorganic filler in the coating liquid is 0-30wt%, including at least one of aluminum hydroxide, aluminum oxide, boehmite, zinc oxide, magnesium oxide, and boron nitride, and the particle size D50 is 0.5-5μm. Different from the aqueous coating liquid, which can be coated in a variety of ways, the uniform solvent-based coating liquid needs to be sprayed to form discontinuous droplets, and then the solvent evaporates to leave a uniform but discontinuous solute to obtain the bonding layer.

[0036] Preferably, the adhesive tape further comprises at least one release layer, which is located on the surface of the porous substrate facing away from the adhesive layer, and / or on the surface of the adhesive layer facing away from the porous substrate. A release agent may be applied on the surface of the porous substrate facing away from the adhesive layer to obtain the release layer, and a release film may be provided on the surface of the adhesive layer facing away from the porous substrate.

[0037] In a second aspect, the present invention provides a method for preparing the aforementioned high-transparency adhesive tape, comprising the following steps:

[0038] Step 1: preparing a thermoplastic coating liquid containing an olefin polymer;

[0039] Step 2: Apply the coating solution to at least one surface of the porous substrate, with a coating amount of 0.01-80 g / m 2 ;

[0040] Step 3: Drying the coating liquid to obtain the high-transparency adhesive tape.

[0041] Among them, the drying method in step three is preferably drying in a drying oven, and the drying oven temperature is controlled at 30-150° C., preferably 50-120° C.; the drying time is 10-300s, preferably 60-180s.

[0042] In the third aspect, the present invention also provides the application of the aforementioned high-transparency tape for lithium battery pole piece protection, negative electrode bonding, pole ear protection, and winding tailing, which is bonded to the joint position by cold pressing or hot pressing. When in use, the tape with a release layer can be directly bonded to the joint position by cold pressing, while the tape without a release layer activates the pressure sensitivity of the adhesive layer by a hot pressing process, and the tape is attached to the position to be joined, such as the position with a large bending amplitude during the winding of the pole piece. The hot pressing temperature is 70-160°C. In the subsequent shaping process, it can effectively prevent the pole piece from cracking and improve the qualified rate of the battery product. The high air permeability of the tape as a whole does not block the transmission of lithium ions. In addition, during the battery cycle, it reduces the problems of lithium precipitation, deformation and fracture of the battery cell corners. In addition, it can also be used for pole piece (edge) protection, pole ear protection, winding tail, etc.

[0043] The present invention has at least the following beneficial effects:

[0044] (1) The present invention applies a polyolefin polymer in the form of a thermoplastic coating liquid onto a breathable porous substrate, and dries it to obtain a uniform but discontinuously distributed adhesive layer. The adhesive tape prepared in this way uses a porous substrate with a relatively high porosity and a discontinuously distributed adhesive layer. On the basis of ensuring sufficient bonding performance and mechanical strength, it achieves the technical effect of good overall air permeability and high lithium ion permeability without affecting the lithium ion transmission in the battery.

[0045] (2) The present invention adopts coating of an aqueous coating liquid or spraying of a solvent-based coating liquid to ultimately obtain a uniform non-continuous adhesive layer, which can effectively avoid the problem that ordinary polyolefin polymers are prone to exhibit self-closing characteristics at high temperatures, resulting in reduced air permeability, and reduces the impact on the overall air permeability and ion permeability of the tape.

[0046] (3) The highly permeable adhesive tape prepared by the present invention can promote the uniform distribution of electrolyte at the edges and corners of the battery, which helps to ensure that all parts inside the battery are fully wetted, thereby improving the ion transmission efficiency and improving the battery's charge and discharge performance. At the same time, it can reduce the problem of local overheating caused by uneven electrolyte distribution. Uniform electrolyte distribution helps to avoid local temperature increases, thereby reducing the risk of thermal runaway and improving the overall safety of the battery.

[0047] (4) The highly permeable adhesive tape prepared by the present invention helps to reduce the uneven stress during the charge and discharge process and reduce the microscopic damage inside the battery. The uniform distribution of electrolyte and ions reduces the possibility of local overcharge or overdischarge, avoids local lithium precipitation, and thus prolongs the battery life. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 It is a structural schematic diagram of a first embodiment of the present invention;

[0049] Figure 2It is a structural schematic diagram of a second embodiment of the present invention;

[0050] Figure 3 It is a schematic structural diagram of a third embodiment of the present invention.

[0051] Reference numerals: 1-porous substrate, 2-adhesive layer, 3-release layer A, 4-release layer B. DETAILED DESCRIPTION

[0052] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.

[0054] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.

[0055] A highly permeable lithium battery tape, comprising a porous substrate 1 and an adhesive layer 2, see attached Figure 1 ,in:

[0056] (i) Porous substrate 1: with a thickness of 5-50 μm and an air permeability of 50-450 s / 100 ml, preferably 50-350 s / 100 ml, comprising at least one of a porous membrane and a non-woven fabric; the porous membrane has a porosity of 30-60% and is selected from at least one of a single-layer PP membrane, a multi-layer PP membrane, a single-layer PE membrane, a multi-layer PE membrane, a PP / PE composite membrane, a PP / PE / PP sandwich membrane, and a PVDF membrane; the non-woven fabric has a pore size of ≤10 μm and is selected from at least one of a PP non-woven fabric, a PE non-woven fabric, a PET non-woven fabric, and a PTFE non-woven fabric.

[0057] (ii) Adhesive layer 2: a non-continuous adhesive layer 2 is formed by coating a thermoplastic coating liquid on at least one surface of the porous substrate 1;

[0058] The thermoplastic coating liquid comprises an olefin polymer and an optional tackifying resin; wherein the olefin polymer has a melting point of 60-150°C and is selected from at least one of polyolefin resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers, ethylene-methacrylic acid copolymers, and polyvinylidene fluoride; and the polyolefin resin is selected from at least one of polypropylene resins, amorphous α-olefin copolymers, ethylene-octene or ethylene-butene copolymers, maleic anhydride grafted polyolefins, acrylic acid grafted polyolefins, methacrylic acid grafted polyolefins, and acrylic acid / methacrylic acid blended modified polyolefins.

[0059] The tackifying resin is selected from at least one of hydrogenated C5, hydrogenated C9 resin, hydrogenated C5 / C9 copolymer resin, hydrogenated DCPD, hydrogenated rosin, and hydrogenated polyterpene resin.

[0060] Thermoplastic coating liquid is 1. water-based coating liquid or 2. solvent-based coating liquid:

[0061] 1. The aqueous coating liquid comprises the following raw materials in parts by weight:

[0062] 98-99.5 parts of aqueous emulsion;

[0063] Inorganic filler 0-40 parts;

[0064] Wetting agent 0-2 parts;

[0065] The solid content of the aqueous emulsion is 1-40%, and emulsion microspheres are dispersed therein, the emulsion microspheres contain the olefin polymer, and the particle size D50 of the emulsion microspheres is 0.2-2 μm;

[0066] The aqueous emulsion also includes 0.01-10wt% of an emulsifier, and optional auxiliary emulsifiers and defoamers; the emulsifier is selected from at least one of C8-C18 higher fatty acid salts, alkyl sulfates, alkyl sulfonates, phosphate esters, polyoxyethylene fatty alcohol ethers, polyoxyethylene alkylphenol ethers with an EO segment ≤ 20, and EO / PO block copolymers with an EO+PO segment of 20-80; the auxiliary emulsifier is selected from C2-C5 short-chain alcohols or polyglycerol esters; the defoamer is selected from one or more of polysiloxane defoamers, silicone emulsion defoamers, polyether defoamers, polyether-modified silicon defoamers, and high-carbon alcohol defoamers.

[0067] The inorganic filler includes at least one of aluminum hydroxide, aluminum oxide, boehmite, zinc oxide, magnesium oxide, and boron nitride, and the particle size D50 is 0.5 to 5 μm;

[0068] The wetting agent includes anionic wetting agent or nonionic wetting agent. Anionic wetting agents include alkyl sulfates, alkyl sulfonates, higher fatty acid salts, phosphate esters, fatty acids or fatty acid sulfate esters; nonionic wetting agents include one or more of polyoxyethylene alkylphenol ethers, polyoxyethylene fatty alcohol ethers, and EO / PO block copolymers, with an HLB value between 5 and 20, preferably 7 to 13.

[0069] The method for preparing the highly permeable lithium battery tape using the aqueous coating liquid comprises the following steps:

[0070] Step 1: preparing an aqueous coating liquid containing an olefin polymer according to the above raw material composition in parts by weight;

[0071] Step 2: Apply the aqueous coating liquid to at least one surface of the porous substrate 1, with a coating amount of 0.01-80 g / m 2 , preferably 0.5-20g / m 2 ; The coating method can be gravure coating, reverse roller coating, wire rod coating, slit coating, air knife coating, curtain coating, spray coating, dip coating, gap coating, etc., wherein the spray coating process does not require the addition of a wetting agent;

[0072] Step 3: Dry the coating liquid, and the solid components are finally attached to the surface of the porous substrate 1 in a substantially uniform but discontinuous manner in the form of microspheres or quasi-spherical structures, thereby obtaining the highly permeable lithium battery tape. The drying device is preferably a drying channel, and the drying channel temperature is controlled at 30 to 150° C., preferably 50 to 120° C.; the drying time is 10 to 300 seconds, preferably 60 to 180 seconds.

[0073] In step 1, the preparation of the aqueous coating liquid can be prepared according to the above raw material ratio and with reference to the existing emulsion preparation technology. Among them, the aqueous emulsion with emulsion microspheres dispersed therein can be prepared by hot melt method, granulation dispersion method, phase inversion method and other processes.

[0074] For example, (1) preparing an aqueous emulsion by hot melt method may include:

[0075] 1) Putting the raw materials of the aqueous emulsion into a pressure reactor according to the formula;

[0076] 2) Add deionized water, alkaline substances, solvents, emulsifiers, etc.; pressurize to 1-15MPa, heat to 90-200℃, and shear at high speed;

[0077] 3) Cooling and discharging to obtain an aqueous emulsion.

[0078] (2) The granulation dispersion method for preparing the aqueous emulsion may include:

[0079] 1) Adding raw materials and solvent into a reactor to dissolve according to the formula ratio;

[0080] 2) The material is dried by spraying equipment to become powder;

[0081] 3) Dispersing emulsifiers and other auxiliary agents and powders in water at high speed to obtain an aqueous emulsion.

[0082] (3) The phase inversion method for preparing an aqueous emulsion may include:

[0083] 1) Put the raw materials into the reactor according to the formula ratio; add the solvent into the reactor and fully dissolve it at 40-150°C;

[0084] 2) adding an emulsifier, an alkaline substance and deionized water into a reaction kettle, stirring and performing high-speed shearing;

[0085] 3) The solvent molecules are removed by distillation equipment to obtain an aqueous emulsion.

[0086] In addition, the particle size of the emulsion microspheres can be controlled by controlling the type and amount of emulsifiers, co-emulsifiers, solvents, etc., as well as process parameters such as heating temperature, high-speed dispersion / shear rate, pressure, time, etc. Then, inorganic fillers, color powder, wetting agents and other components are added as needed to prepare a water-based coating liquid.

[0087] 2. A solvent-based coating liquid, comprising the olefin polymer, a solvent and an optional inorganic filler, wherein the concentration of the olefin polymer is 5-20 wt %. The solvent-based coating liquid is sprayed to form the discontinuous adhesive layer 2.

[0088] The solvent is selected from at least one of aromatic hydrocarbon solvents, ketone solvents and aliphatic hydrocarbon solvents. The mass concentration of the inorganic filler in the coating liquid is 0-30%, including at least one of aluminum hydroxide, aluminum oxide, boehmite, zinc oxide, magnesium oxide and boron nitride, and the particle size D50 is 0.5-5 μm;

[0089] The method for preparing the highly transparent lithium battery tape using the solvent-based coating liquid comprises the following steps:

[0090] Step 1: preparing a solvent-based coating solution containing an olefin polymer;

[0091] Step 2: Spray the solvent-based coating liquid onto at least one surface of the porous substrate 1, with a spraying amount of 0.01-80 g / m 2 , preferably 0.5-20g / m 2 ;

[0092] Step 3: Dry the coating liquid, and as the solvent evaporates, the solute precipitates and is basically uniformly but discontinuously attached to the surface of the porous substrate 1, thereby obtaining the highly permeable lithium battery tape. The drying device is preferably a drying channel, and the drying channel temperature is controlled at 30-150°C, preferably 50-120°C; the drying time is 10-300s, preferably 60-180s.

[0093] (iii) An optional release layer is located on the surface of the porous substrate 1 facing away from the adhesive layer 2, and / or located on the surface of the adhesive layer 2 facing away from the porous substrate 1. For example, a release agent can be applied to the surface of the porous substrate 1 facing away from the adhesive layer 2 to obtain a release layer A3, see the attached Figure 2 A release film may be provided on one side of the adhesive layer 2 facing away from the porous substrate 1 to obtain a release layer B 4, see attached Figure 3 .

[0094] Example 1

[0095] A highly permeable lithium battery tape comprises a porous substrate and an adhesive layer, wherein

[0096] (1) Porous substrate: A PP membrane with a thickness of 20 μm, an air permeability of 180 s / 100 ml, and a porosity of 50 ± 10% was selected as the substrate;

[0097] (2) Adhesive layer: A discontinuous adhesive layer is formed by coating a thermoplastic coating liquid on one surface of the porous substrate; the thermoplastic coating liquid is an aqueous coating liquid, and comprises the following raw materials in parts by weight:

[0098] Aqueous emulsion 99 parts;

[0099] 1 part wetting agent;

[0100] The solid content of the aqueous emulsion is 3%, and emulsion microspheres are dispersed therein. The emulsion microspheres contain an olefin polymer, and the olefin polymer is maleic anhydride grafted polypropylene (brand number Polinker PL2480). The particle size D50 of the emulsion microspheres is about 0.3 μm, and the melting point is about 85° C.

[0101] Prepared by the following method:

[0102] Step 1: configure the above parameters of polyolefin thermoplastic coating liquid;

[0103] Step 2: Apply the coating solution to one surface of the porous substrate using a gravure coating method, with a coating amount of 0.18 g / m 2 ;

[0104] Step 3: Dry the coating liquid in a drying channel at a drying temperature of 60-80° C. and a drying time of 60 seconds to obtain the highly transparent lithium battery tape.

[0105] Example 2

[0106] The difference between this embodiment and embodiment 1 is that the solid content of the aqueous emulsion used in this embodiment is 8%, and the coating amount of the coating liquid is 0.98 g / m 2 .

[0107] Example 3

[0108] The difference between this embodiment and embodiment 1 is that the solid content of the aqueous emulsion used in this embodiment is 20%, and the coating amount of the coating liquid is 16.6 g / m 2 .

[0109] Example 4

[0110] The difference between this embodiment and embodiment 1 is that the solid content of the aqueous emulsion used in this embodiment is 30%, and the coating amount of the coating liquid is 26.3 g / m 2 .

[0111] Example 5

[0112] The difference between this embodiment and embodiment 3 is that the particle size D50 of the emulsion microspheres in the aqueous emulsion used in this embodiment is about 0.5 μm, and the coating amount of the coating liquid is 16.4 g / m 2 .

[0113] Example 6

[0114] The difference between this embodiment and embodiment 3 is that the particle size D50 of the emulsion microspheres in the aqueous emulsion used in this embodiment is about 1.3 μm, and the coating amount of the coating liquid is 17.2 g / m 2 .

[0115] Example 7

[0116] The difference between this embodiment and embodiment 3 is that the particle size D50 of the emulsion microspheres in the aqueous emulsion used in this embodiment is about 1.8 μm, and the coating amount of the coating liquid is 17.3 g / m 2 .

[0117] Example 8

[0118] The difference between this embodiment and embodiment 6 is that the coating amount of the coating liquid in this embodiment is 16.7 g / m 2 , the drying temperature of the drying channel is set to 80-100℃.

[0119] Example 9

[0120] The difference between this embodiment and embodiment 6 is that the coating amount of the coating liquid in this embodiment is 16.7 g / m 2 , the drying time of the drying channel is set to 180s.

[0121] Example 10

[0122] The difference between this embodiment and embodiment 6 is that the coating amount of the coating liquid in this embodiment is 16.9 g / m 2 , the drying time of the drying channel is set to 300s.

[0123] Embodiment 11

[0124] The difference between this embodiment and embodiment 6 is that the olefin polymer contained in the latex microspheres in this embodiment is maleic anhydride grafted polypropylene (brand name PolinkerPL2400), the melting point is about 60°C, and the coating amount of the coating liquid is 16.6 g / m 2 .

[0125] Example 12

[0126] The difference between this embodiment and embodiment 6 is that the olefin polymer contained in the latex microspheres in this embodiment is maleic anhydride grafted polypropylene (brand name Fusabond P353), the melting point is 100°C, and the coating amount of the coating liquid is 17.2 g / m 2 .

[0127] Embodiment 13

[0128] The difference between this embodiment and embodiment 6 is that the olefin polymer contained in the latex microspheres in this embodiment is maleic anhydride grafted polypropylene (brand Exxelor PO 1015 + Polinker PL2400 mixture), the melting point is 120 ° C, and the coating amount of the coating liquid is 17.0 g / m 2 .

[0129] Embodiment 14

[0130] The difference between this embodiment and embodiment 6 is that the olefin polymer contained in the latex microspheres in this embodiment is maleic anhydride grafted polypropylene (brand name Exxelor PO 1015), the melting point is about 140°C, and the coating amount of the coating liquid is 16.8 g / m 2 .

[0131] Embodiment 15

[0132] The difference between this embodiment and embodiment 3 is that the embodiment uses a 9 μm PP diaphragm substrate, the air permeability of the substrate is 120 s / 100 ml, and the coating amount of the coating liquid is 16.5 g / m 2 .

[0133] Example 16

[0134] The difference between this embodiment and embodiment 3 is that the present embodiment uses a 45 μm PP diaphragm substrate, the substrate air permeability is 280 s / 100 ml, and the coating amount of the coating liquid is 16.6 g / m 2 .

[0135] Embodiment 17

[0136] The difference between this embodiment and embodiment 3 is that the embodiment uses a 20 μm PP non-woven fabric substrate with a pore size of ≤10 μm, a substrate air permeability of 220 s / 100 ml, and a coating amount of 16.5 g / m 2 .

[0137] Embodiment 18

[0138] The difference between this embodiment and embodiment 3 is that the embodiment uses a 9 μm PP non-woven fabric substrate with a pore size of ≤10 μm, a substrate air permeability of 130 s / 100 ml, and a coating amount of 16.8 g / m 2 .

[0139] Embodiment 19

[0140] The difference between this embodiment and embodiment 3 is that the embodiment uses a 45 μm PP non-woven fabric substrate with a pore size of ≤10 μm, a substrate air permeability of 300 s / 100 ml, and a coating amount of 16.4 g / m 2 .

[0141] Comparative Example 1

[0142] The difference between Comparative Example 1 and Example 3 is that a 60 μm PP diaphragm substrate is used, the porosity is 50±10%, and the air permeability of the substrate is 370 s / 100 ml.

[0143] Comparative Example 2

[0144] The difference between Comparative Example 2 and Example 3 is that the coating amount of the coating liquid is about 85g / m 2 The drying temperature of the drying channel is set to 80-100℃ and the drying time is 180s.

[0145] Embodiment 20

[0146] The difference between this embodiment and embodiment 6 is that the EVA emulsion microspheres are used in this embodiment. The melting point of EVA (brand UL 15019CC) is about 85°C, and the coating amount of the coating liquid is 16.3 g / m 2 .

[0147] Embodiment 21

[0148] A highly permeable lithium battery tape comprises a porous substrate and an adhesive layer, wherein

[0149] (1) Porous substrate: A PP membrane with a thickness of 20 μm, an air permeability of 180 s / 100 ml, and a porosity of 50 ± 10% was selected as the substrate;

[0150] (2) Adhesive layer: A non-continuous adhesive layer is formed by coating a thermoplastic coating liquid on one surface of the porous substrate; the thermoplastic coating liquid is a NMP solution (solvent-based coating liquid) of PVDF (brand name Solef11010) with a concentration of 12% and a melting point of 140° C.

[0151] Prepared by the following method:

[0152] Step 1: configure the above parameters of polyolefin thermoplastic coating liquid;

[0153] Step 2: Spray the coating solution onto one surface of the porous substrate with a coating amount of 17.4 g / m 2 ;

[0154] Step 3: Dry the coating liquid in a drying channel at a drying temperature of 100-120° C. and a drying time of 180 seconds to obtain the highly transparent lithium battery tape.

[0155] Embodiment 22

[0156] The difference between this embodiment and embodiment 21 is that this embodiment uses a 9 μm PP diaphragm substrate with an air permeability of 120s / 100ml.

[0157] Embodiment 23

[0158] The difference between this embodiment and embodiment 21 is that this embodiment uses a 45 μm PP diaphragm substrate with an air permeability of 280 s / 100 ml.

[0159] Embodiment 24

[0160] The difference between this embodiment and embodiment 21 is that this embodiment uses a 20 μm PP non-woven fabric substrate with an air permeability of 220s / 100ml.

[0161] Embodiment 25

[0162] The difference between this embodiment and embodiment 21 is that the solvent-based coating liquid used in this embodiment is a methyl isobutyl ketone (MIBK)-methylcyclohexane solution of POE (brand name Vistamaxx 3588FL) with a concentration of 10% and a melting point of about 85°C; the coating amount is 17.1 g / m 2 ; The drying temperature in the drying channel is 60-80℃, and the drying time is 60s.

[0163] Comparative Example 3

[0164] The difference between Comparative Example 3 and Example 21 is that a 60 μm PP diaphragm substrate is used, the porosity is 50±10%, and the air permeability of the substrate is 370 s / 100 ml.

[0165] Comparative Example 4

[0166] The difference between Comparative Example 4 and Example 21 is that the coating amount of the coating liquid is about 85g / m 2 The drying temperature of the drying channel is set to 100-120℃ and the drying time is 300s.

[0167] The coating liquid and process parameters of each embodiment and comparative example are shown in Table 1:

[0168] Table 1

[0169]

[0170]

[0171] Test method:

[0172] (1) Peel strength test method - before soaking

[0173] Test method: Clean the aluminum foil to be tested with isopropyl alcohol and dry it, cut the tape sample into strips with a width of 24mm and a length of 100mm; align the test surface of the tape strip with the aluminum foil to be tested, press at 95℃ and 0.2Mpa for 1s to avoid bubbles or wrinkles; stick the back of the aluminum foil (the side without tape) to the stainless steel plate with double-sided tape, start the timer, and maintain for 20min; fix one end of the stainless steel plate on the lower fixture of the tensile machine and make it perpendicular to the horizontal plane, and reset the equipment; clamp the substrate of the tape strip with another fixture, and perform a peel test at a speed of 304.8mm / min, and select a section with stable data (not shorter than 80mm) to calculate the peel strength in N / mm.

[0174] (2) Peel strength test method - after soaking

[0175] Test method: Prepare the tape sample according to the method of test (1), put it into a container containing electrolyte solvent after curing, ensure that the liquid surface completely immerses the sample, bake it at 85°C for 24 hours, take it out and wipe off the surface solvent, and test the peel strength after leaving it for 20 minutes using the method of test 1. The electrolyte solvent contains ethylene carbonate EC 20wt%, ethyl methyl carbonate EMC 50wt% and ethyl propionate EP 30wt%.

[0176] (3) Air permeability test method

[0177] Cut the tape sample into a circular film with a diameter of >10cm or a square film with a side length of >10cm; turn on the device, hold the slide against the top of the slide; rotate the slide, and make the infrared probe perpendicular to the central axis of the 100ml test area; place the film to be tested on the test seat and tighten it; the screen displays "TIMER SEEKING STARTING MARK", press the "RESET" key and release the slide to start the test. After the test is completed, read the value on the screen in s / 100ml.

[0178] (4) High temperature aging air permeability test

[0179] Cut the tape sample into a circle with a diameter of >10 cm or a square with a side length of >10 cm, bake it at 110°C for 24 hours, take it out, cool it to room temperature, and test the air permeability according to the test method of test (3).

[0180] (5) Air permeability test after soaking

[0181] Cut the tape sample into a circular film with a diameter of >10cm or a square film with a side length of >10cm, put it into a container containing electrolyte solvent, ensure that the liquid surface completely immerses the film, bake it at 85℃ for 24h, take it out and wipe off the surface solvent, leave it for 20min, and test the air permeability according to the test method of test 3. The electrolyte solvent contains ethylene carbonate EC 20wt%, ethyl methyl carbonate EMC 50wt% and ethyl propionate EP 30wt%.

[0182] The test results are shown in Table 2:

[0183] Table 2

[0184]

[0185]

[0186] After a lot of experimental exploration and optimization, the initial air permeability of the adhesive tape of the present invention is P1≤2.5×P0, where P0 is the air permeability of the porous substrate, which is 50-450s / 100ml, preferably 50-350s / 100ml.

[0187] After high temperature aging of the tape (for example, after baking at 110°C for 24 hours, take it out and cool it to room temperature for testing), the air permeability of the tape is P2≤4.0×P1, preferably P2≤2.5×P1, and more preferably the air permeability of the tape satisfies: P2=A h ×P1-B h , where A h The value is 1.2-2.2, B h The value range is 0-30;

[0188] After the tape is soaked in electrolyte (for example, completely immersed in the electrolyte solvent, baked at 85°C for 24 hours, taken out, wiped clean and left for 20 minutes before testing, the electrolyte solvent contains ethylene carbonate EC 20wt%, ethyl methyl carbonate EMC 50wt% and ethyl propionate EP 30wt%), the air permeability of the tape P3≤1.2×P1; preferably, the air permeability of the tape P3 satisfies: P3=A e ×P1+B e , where A e The value is 1.02-1.1, B e The value range is 0-15.

[0189] The present invention selects a porous substrate with good permeability and cooperates with a suitable adhesive layer to obtain a lithium battery tape with excellent air permeability, air permeability after high-temperature aging and air permeability after soaking in electrolyte. Under the premise of not affecting the passage of lithium ions, it can protect the electrode from cracking under stress during the hot pressing process and prevent lithium deposition in the battery during the battery cycle, which is beneficial to improving the safety of battery use and extending the battery life.

[0190] By comparing the compositions and test results of the embodiments and comparative examples, it can be seen that there are multiple options for the porous substrate and the adhesive layer, but both can basically meet the requirements of air permeability and adhesion and meet the application scenarios of the tape under the conditions of meeting the aforementioned preset material selection methods and test results. Even if the individual parameters of comparative examples 1-4 meet the requirements, they still cannot take into account the comprehensiveness required by the lithium battery tape as a whole.

[0191] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the technical solution of the present invention is intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention.

Claims

1. A high-transparency adhesive tape, characterized in that: including a laminated porous substrate and an adhesive layer; The porous substrate has a thickness of 5-50 μm and an air permeability of 50-450 s / 100 ml, and includes at least one of a porous membrane and a non-woven fabric; The adhesive layer is formed by coating a thermoplastic coating liquid on at least one surface of the porous substrate to form a discontinuous adhesive layer; the thermoplastic coating liquid is an aqueous coating liquid or a solvent-based coating liquid, comprising an olefin polymer and an optional tackifying resin, and the coating amount is 0.01-80 g / m 2 The olefin polymer has a melting point of 60-150°C and is selected from at least one of polyolefin resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methyl acrylate copolymers, and ethylene-methacrylic acid copolymers; The aqueous coating solution comprises the following raw materials in parts by weight: 98-99.5 parts of aqueous emulsion; Inorganic filler 0-40 parts; Wetting agent 0-2 parts; The solid content of the aqueous emulsion is 1-40%, and emulsion microspheres are dispersed therein, the emulsion microspheres contain the olefin polymer, and the particle size D50 of the emulsion microspheres is 0.2-2 μm; The solvent-based coating liquid comprises the olefin polymer, a solvent and an optional inorganic filler, the concentration of the olefin polymer is 5-20wt%, and the solvent-based coating liquid forms the discontinuous adhesive layer by spraying; The initial air permeability of the tape is P1≤2.5×P0, where P0 is the air permeability of the porous substrate; After high temperature aging, the air permeability of the tape is P2≤4.0×P1; After soaking in electrolyte, the air permeability of the tape is P3≤1.2×P1.

2. The high-transparency adhesive tape according to claim 1, characterized in that: The tackifying resin is selected from at least one of hydrogenated C5, hydrogenated C9 resin, hydrogenated C5 / C9 copolymer resin, hydrogenated DCPD, hydrogenated rosin, and hydrogenated polyterpene resin.

3. The high-transparency adhesive tape according to claim 1, characterized in that: The polyolefin resin is selected from at least one of polypropylene resin, amorphous α-olefin copolymer, ethylene-octene or ethylene-butene copolymer, maleic anhydride grafted polyolefin, acrylic acid grafted polyolefin, methacrylic acid grafted polyolefin, acrylic acid / methacrylic acid blended modified polyolefin.

4. The high-transparency adhesive tape according to any one of claims 1 to 3, characterized in that: The porous substrate comprises a porous membrane with a porosity of 30-60%, selected from at least one of a single-layer PP membrane, a multi-layer PP membrane, a single-layer PE membrane, a multi-layer PE membrane, a PP / PE composite membrane, a PP / PE / PP sandwich membrane, and a PVDF membrane; and / or The porous substrate comprises a non-woven fabric with a pore size of ≤10 μm, and is selected from at least one of PP non-woven fabric, PE non-woven fabric, PET non-woven fabric, and PTFE non-woven fabric.

5. The high-transparency adhesive tape according to claim 4, characterized in that: In the aqueous coating liquid, the inorganic filler includes at least one of aluminum hydroxide, aluminum oxide, boehmite, zinc oxide, magnesium oxide, and boron nitride, and the particle size D50 is 0.5-5 μm; The wetting agent includes anionic wetting agents or nonionic wetting agents.

6. The high-transparency adhesive tape according to claim 5, characterized in that: The aqueous emulsion also includes 0.01-10wt% of an emulsifier, and optionally an auxiliary emulsifier and a defoamer; The emulsifier is selected from at least one of C8-C18 higher fatty acid salts, alkyl sulfates, alkyl sulfonates, phosphate esters, polyoxyethylene fatty alcohol ethers, polyoxyethylene alkylphenol ethers with EO segments ≤ 20, and EO / PO block copolymers with EO+PO segments of 20-80.

7. The high-transparency adhesive tape according to claim 5 or 6, characterized in that: The invention also comprises at least one release layer, wherein the release layer is laminated on the surface of the porous substrate facing away from the adhesive layer and / or laminated on the surface of the adhesive layer facing away from the porous substrate.

8. A method for preparing the highly transparent adhesive tape according to any one of claims 1 to 7, characterized in that: The steps include: Step 1: preparing a thermoplastic coating liquid containing an olefin polymer; Step 2: Apply the coating solution to at least one surface of the porous substrate, with a coating amount of 0.01-80 g / m 2 ; Step 3: Drying the coating liquid to obtain the high-transparency adhesive tape.

9. Application of the high-transparency adhesive tape according to any one of claims 1 to 7 for lithium battery pole piece protection, negative electrode bonding, pole ear protection, and winding and finishing, characterized in that: Bonded to the joint by cold or hot pressing.