A production process for superconducting wire and superconducting enameled wire

By using the technology of combining a constant-temperature paint chamber and a constant-temperature chamber in the superconducting wire production process, the problem of paint adhesion caused by temperature mismatch is solved, the uniformity and fluidity control of the paint film thickness are achieved, and the product qualification rate is improved. and adaptability, ensuring the stable performance of superconducting wires.

CN118197707BActive Publication Date: 2024-10-15GUANGDONG JINGDA REA SPECIAL ENAMELED WIRE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410618798.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-15
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

In the existing superconducting wire production process, temperature mismatch leads to insufficient adhesion or poor fluidity of the paint liquid, which easily forms pinholes and bumps, resulting in high product rejection rates. It is also unable to cope with temperature changes in the production environment throughout the seasons, affecting product quality.

Method used

Using a process that combines a constant-temperature painting chamber and a constant-temperature chamber, the core wire is run at a constant speed and the temperature is fixed before each painting, so that the temperature of the core wire matches the temperature of the paint liquid to ensure uniform thickness of the paint film and no pinholes. Painting and baking are repeated, combined with a fixed-thickness mold and a spray paint tube, to control the thickness and fluidity of the paint film, identify the wiring position and record real-time process data.

Benefits of technology

It achieves precise control of the paint film thickness, reduces pinholes and unevenness, improves product qualification rate, adapts to temperature changes in four seasons, and ensures the performance stability and quality of superconducting wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118197707B_ABST
    Figure CN118197707B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of superconducting wires, and in particular to a production process of superconducting wires and superconducting enameled wires. The process comprises the following steps: pay-off; forming: rolling the future round wire into a core wire of set specifications; cleaning: cleaning the formed core wire; annealing: the core wire running at a constant speed is annealed in an annealing furnace; painting and baking: the core wire running at a constant speed enters a constant temperature painting room for painting and then enters a baking furnace for baking, and the painting and baking are repeated 6 to 10 times; the core wire is set at a constant temperature before each painting; detection: the core wire after the painting and baking is detected; winding: winding the core wire into a finished product bobbin. In the production process of the superconducting wire of the present invention, the core wire enters a constant temperature painting room at a set temperature for painting, ensuring that the thickness of the insulating paint film is uniform and free of pinholes and bumps, thereby improving the product qualification rate. The superconducting enameled wire is prepared by the above-mentioned production process of the superconducting wire, and the insulating paint layer is uniform, free of pinholes and bumps, and has stable performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of superconducting wires, and in particular to a production process of superconducting wires and superconducting enameled wires. Background Art

[0002] Enameled wire is widely used in electrical equipment. When the enameled wire is painted, the wire continuously passes through the pay-off equipment, core wire forming equipment, annealing equipment, painting equipment, testing equipment and winding equipment. After the wire spool of the pay-off equipment is finished, the fully loaded spool is quickly replaced, and the front and rear wires are welded together to achieve continuous painting. In the winding equipment, after a spool is fully loaded, the wire is cut, and the empty spool is replaced and rewound. The core wire of the conventional enameled wire is copper wire, aluminum wire, copper-clad aluminum or aluminum-clad copper. The core wire material is single or the structure is simple. The core wire welding position in the enameled wire has little effect on the performance of the enameled wire. Therefore, the existing enameled wire production process usually adopts the method of thin paint multiple coatings to cover the core wire with an insulating paint layer.

[0003] Superconducting wires are used in medical equipment, laboratory instruments, superconducting energy storage, maglev trains and other fields. The core wire of the superconducting wire is required to be continuous and uniform in thickness. In particular, the superconducting wire used to make coils requires a uniform thickness of the insulating paint layer of the superconducting wire to ensure that each coil of the wire is closely arranged without gaps. In addition, the insulating paint layer of the superconducting wire must be free of pinholes and bumps to ensure the performance of the superconducting wire.

[0004] In the existing superconducting wire production process, the annealed wire and the baked wire are directly painted. According to research, if the wire temperature is too high, the amount of paint liquid attached to the wire is small, and pinholes are easily formed. If the wire temperature is too low, the attached paint liquid has poor fluidity and is prone to unevenness. If pinholes or unevenness appear in the insulating paint layer of the superconducting wire, the entire superconducting wire will be scrapped, and the scrap rate of superconducting wire painting is high.

[0005] In addition, pinholes are likely to occur when the temperature of the paint liquid does not match the temperature of the bare wire. The existing technology does not control the temperature of the paint liquid and the bare wire, making it unable to cope with the temperature changes in the production environment throughout the four seasons. The temperature of the paint liquid and the bare wire fluctuates throughout the year, and the product quality is unstable. Summary of the invention

[0006] The purpose of the present invention is to provide a production process for superconducting wires, wherein the core wire enters a constant temperature painting room at a set temperature for painting, ensuring that the insulating paint film has a uniform thickness and is free of pinholes and bumps, and the production process copes with temperature changes in the production environment and improves the product qualification rate;

[0007] Another object of the present invention is to provide a superconducting enameled wire, the insulating varnish layer of which is uniform, has no pinholes or bumps, and has stable performance.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] A production process for a superconducting wire comprises the following steps:

[0010] (1) Paying off the line;

[0011] (2) Forming: Rolling the incoming round wire into a core wire of set specifications;

[0012] (3) Cleaning: Clean the formed core wire;

[0013] (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace;

[0014] (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room for painting and then enters the baking furnace for baking. The painting and baking are repeated 6 to 10 times. The core wire is kept at a constant temperature before each painting so that the temperature of the core wire matches the temperature of the paint liquid.

[0015] (6) Inspection: inspect the core wire after painting and baking;

[0016] (7) Winding: Wind the core wire onto the finished spool.

[0017] Furthermore, in step (5), the temperature at which the core wire is kept constant is higher than the temperature of the constant temperature paint room, the constant temperature paint room has a paint trough for receiving excess paint liquid, the core wire passes through the paint trough and runs upward through the thickness setting mold, a paint spraying tube is provided between the paint trough and the thickness setting mold, and the temperature of the paint liquid sprayed from the paint spraying tube is the same as the temperature in the constant temperature paint room.

[0018] Furthermore, the temperature of the paint liquid in the paint tank and the temperature in the constant temperature painting room are both 40°C to 45°C;

[0019] The temperature at which the core wire is kept constant is 2°C to 5°C higher than the temperature of the constant temperature painting room.

[0020] Furthermore, in the step (5), the thickness of the paint film formed by each painting is the same, and the thickness of the paint film formed by each painting is 10 μm to 80 μm.

[0021] Furthermore, the core wire is kept at a constant temperature in a constant temperature chamber, and the constant temperature chamber is connected to the constant temperature painting chamber so that the core wire enters the constant temperature painting chamber from the constant temperature chamber;

[0022] The length of the temperature-regulating chamber is greater than 20 cm. The temperature-regulating chamber is divided into a cooling chamber and a constant temperature chamber. The core wire first enters the cooling chamber and then enters the constant temperature chamber.

[0023] Furthermore, in the step (1), each pay-off shaft is wound with a superconducting wire, and two adjacent superconducting wires are welded to form a connection point;

[0024] Each of the steps (2) to (7) has a wiring position identification step to identify the wiring position as a process node and record the real-time process data of each superconducting wire;

[0025] In the step (7), the core wire is cut according to the connection position so that each superconducting wire is wound on a finished product spool.

[0026] Furthermore, in the step (1), two adjacent superconducting wires are welded with ferromagnetic material to form a connection point, and a joint identification mechanism is used to identify the connection point;

[0027] The joint identification mechanism includes a pressure sensor and a strong magnet connected to each other. The strong magnet is used to generate suction force on the joint to change the sensing data of the pressure sensor.

[0028] Furthermore, in the step (5), acetal insulating varnish is used, the baking time is 40 s to 80 s, and the baking temperature is 260° C. to 300° C.

[0029] Furthermore, in the step (4), the annealing temperature is 280°C to 320°C, and the annealing time is 80 s to 100 s.

[0030] A superconducting enameled wire is prepared by adopting the above-mentioned production process of superconducting wire.

[0031] The technical solution provided by the present invention may include the following beneficial effects:

[0032] 1. The superconducting wire, which will be a round wire in the future, will be made into a core wire and then coated with insulating paint. By limiting the uniform speed of the core wire, setting the temperature before painting the core wire, and painting the core wire multiple times, the thickness of the paint film can be accurately controlled, so that the production process can cope with the temperature changes in the production environment in four seasons, ensuring that the paint film has no pinholes and bumps, greatly improving the quality of the product.

[0033] 2. By identifying the wiring position, the real-time process data of each superconducting wire can be recorded with the wiring position identified as the process node; it can also ensure that each superconducting wire is wound on a finished product spool.

[0034] 3. Making the temperature of the core wire slightly higher than the temperature of the constant temperature paint room can not only achieve the effect of accelerating the flow to the paint tank, but the excess heat of the core wire also helps to maintain the temperature in the constant temperature paint room, without the need to frequently start the heating element to compensate for the temperature of the constant temperature paint room. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a flowchart of a process for producing a superconducting wire according to an embodiment of the present invention. DETAILED DESCRIPTION

[0036] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0037] Combine the following Figure 1 , describing a production process of a superconducting wire and a superconducting enameled wire according to an embodiment of the present invention.

[0038] A production process for a superconducting wire comprises the following steps:

[0039] (1) Paying off the line;

[0040] (2) Forming: Rolling the incoming round wire into a core wire of set specifications;

[0041] (3) Cleaning: Clean the formed core wire;

[0042] (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace;

[0043] (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room for painting and then enters the baking furnace for baking. The painting and baking are repeated 6 to 10 times. The core wire is kept at a constant temperature before each painting so that the temperature of the core wire matches the temperature of the paint liquid.

[0044] (6) Inspection: inspect the core wire after painting and baking;

[0045] (7) Winding: Wind the core wire onto the finished spool.

[0046] In the present invention, the superconducting wire which is a round wire is made into a core wire and then coated with insulating paint. By limiting the core wire to run at a uniform speed, keeping the core wire at a constant temperature before painting, and painting the core wire multiple times, the thickness of the paint film can be accurately controlled, so that the production process can cope with the temperature changes in the production environment in four seasons, ensuring that the paint film has no pinholes and bumps, and greatly improving the quality of the product.

[0047] Specifically, in step (4) and step (5), the core wire is made to run at a uniform speed. By strictly controlling the running speed of the core wire, the annealing time and baking time of the core wire can be accurately controlled. The annealed core wire has a uniform softness and can enter the paint room straight, thereby improving the uniformity of the paint film thickness; the accurate baking time makes the paint film have good softness and can be painted again.

[0048] Paint the core wire in the constant temperature painting room to further improve the uniformity of the paint film thickness. In the constant temperature painting room, the fluidity of the paint liquid sprayed from the nozzle and the paint liquid attached to the core wire is consistent, and when passing through the thickness setting die, the excess paint liquid on the core wire can smoothly flow to the paint tank at the bottom of the constant temperature painting room to prevent the uneven paint film phenomenon caused by the difference in paint liquid fluidity. The uneven paint film phenomenon refers to the convexity on the surface of the paint film that makes the paint film thicker or the concaveness of the paint film that makes the paint film thinner. The length of the uneven part of the paint film is generally 0.1mm~10mm.

[0049] It is understandable that the temperature of the core wire after annealing and baking is high and much higher than the temperature of the paint liquid, and the distance between the annealing furnace and the baking furnace and the constant temperature painting room is limited. After research, it is found that the core wire still has a high temperature when entering the constant temperature painting room, and the temperature of the core wire cannot correspond to the temperature of the paint liquid. In addition, the temperature of the core wire entering the painting room in the prior art is not controlled, so that it cannot cope with the temperature changes in the production environment in four seasons. The temperature of the paint liquid and the bare core wire fluctuates throughout the year, the product quality is unstable, and pinholes often occur. At present, the manufacturer requires the number of pinholes per shaft of enameled wire to be less than 10. In the present invention, the core wire is set at a constant temperature before entering the constant temperature painting room, that is, the core wire is cooled to a certain temperature to prevent the core wire temperature from being too high or too low, thereby eliminating the pinhole phenomenon of the paint film and ensuring the qualified rate of superconducting wire painting.

[0050] In one embodiment of the present invention, in step (5), the temperature at which the core wire is kept constant is higher than the temperature of the constant temperature painting room, the constant temperature painting room is provided with a paint trough for receiving excess paint liquid, the core wire passes through the paint trough and runs upward through the thickness setting mold, a paint spraying tube is provided between the paint trough and the thickness setting mold, and the temperature of the paint liquid sprayed out of the paint spraying tube is the same as the temperature in the constant temperature painting room.

[0051] The temperature at which the core wire is set is limited to be higher than the temperature of the constant temperature paint room, so that the paint liquid attached to the core wire can fall into the paint tank more quickly when the core wire first enters the constant temperature paint room. The core wire is a metal wire with a fast heat dissipation speed, and can quickly transfer heat to excess paint liquid. The temperature of the core wire when passing through the paint spray tube can be the same as the temperature of the paint liquid, ensuring that the paint liquid can evenly adhere to the surface of the core wire.

[0052] In one embodiment of the present invention, the paint liquid temperature in the paint tank and the temperature in the constant temperature painting room are both 40°C~45°C; the temperature of the core wire is set at 2°C~5°C higher than the temperature of the constant temperature painting room, so that the temperature of the core wire is slightly higher than the temperature of the constant temperature painting room, which can not only achieve the effect of accelerating the flow of excess paint liquid to the paint tank, but the excess heat of the core wire also helps to maintain the temperature in the constant temperature painting room, and there is no need to frequently start the heating element to compensate for the temperature of the constant temperature painting room.

[0053] In one embodiment of the present invention, in step (5), the thickness of the paint film formed by each painting is the same, and the thickness of the paint film formed by each painting is 10μm~80μm. Through the above-mentioned restriction on the running speed of the core wire, constant temperature painting and core wire constant temperature, the thickness of the paint film can be accurately controlled, and then the insulation performance of the paint film can be accurately controlled. A smaller paint film thickness and a fewer number of painting can meet the insulation requirements, which can not only save the amount of insulating paint and reduce the total thickness of the paint film, but also save baking energy and simplify the structure of the painting equipment based on a fewer number of painting. Preferably, based on acetal insulating paint, the thickness of the paint film formed by each painting is 20μm, and the number of paint baking times is 6 times.

[0054] It should be noted that if the thickness of the paint film formed by each painting is the same, multiple core wires can be baked in the same baking oven, simplifying the baking oven structure.

[0055] In one embodiment of the present invention, the core wire is kept at a constant temperature in a constant temperature chamber, and the constant temperature chamber is connected to a constant temperature painting chamber so that the core wire enters the constant temperature painting chamber from the constant temperature chamber, thereby ensuring the temperature of the core wire entering the constant temperature painting chamber;

[0056] The length of the constant temperature chamber is greater than 20 cm, and the constant temperature chamber is divided into a cooling chamber and a constant temperature chamber. The core wire first enters the cooling chamber and then enters the constant temperature chamber.

[0057] By setting a longer temperature chamber, the core wire can reach the set temperature. Since the core wire enters the temperature chamber directly from the annealing furnace or baking furnace, the temperature of the core wire is relatively high at the beginning of entering the temperature chamber. It first passes through the cooling chamber to cool down and then enters the constant temperature chamber to stabilize the temperature of the core wire, ensuring that the core wire can accurately reach the set temperature. Exemplarily, the cooling chamber cools the core wire by air cooling, and the constant temperature chamber and the constant temperature painting room are both equipped with air conditioners.

[0058] In one embodiment of the present invention, in step (1), each pay-off spool is wound with a superconducting wire, and two adjacent superconducting wires are welded to form a connection position to achieve continuous painting;

[0059] Each of steps (2) to (7) has a wiring position identification step to identify the wiring position as a process node and record the real-time process data of each superconducting wire;

[0060] In step (7), the core wire is cut according to the connection position so that each superconducting wire is wound on a finished product bobbin, thereby ensuring that each superconducting wire is wound on a finished product bobbin.

[0061] The real-time process data of each superconducting wire is recorded by identifying the connection position as the process node, which is convenient for traceability. Since each finished spool is wound with a superconducting wire, each spool has traceability data, which is convenient for data storage. If quality problems are found in the inspection of superconducting wires before application, the cause of the problem can be found through traceability and the quality of products in the same batch can be verified.

[0062] In one embodiment of the present invention, in step (1), two adjacent superconducting wires are welded with ferromagnetic material to form a connection point, and a joint identification mechanism is used to identify the connection point;

[0063] The joint identification mechanism includes a pressure sensor and a strong magnet connected to each other. The strong magnet is used to generate suction to the joint to change the sensing data of the pressure sensor.

[0064] Based on the ferromagnetic material welding to form the joint, when the joint passes through the strong magnet, the strong magnet generates attraction to the joint, and when the pressure sensor is located at the bottom of the strong magnet and the joint passes through the top of the strong magnet, the pressure value detected by the pressure sensor changes, and the joint can be accurately identified. Preferably, two adjacent superconducting wires are welded to form a joint through ferromagnetic material with iron wire as a connecting piece, which can improve the sensitivity of joint identification.

[0065] In one embodiment of the present invention, in step (5), acetal insulating varnish is used, the baking time is 40 s to 80 s, and the baking temperature is 260°C to 300°C to ensure that the curing is sufficient and the paint film is soft. If the baking time is too long and the temperature is too high, the paint film will age and harden and will not be easy to paint again. If the baking time is short and the temperature is low, the paint film cannot be completely cured, and the product paint film is prone to unevenness.

[0066] In one embodiment of the present invention, in step (4) of the production process, the annealing temperature is 280°C to 320°C, and the annealing time is 80 s to 100 s. As the annealing temperature of the superconducting material in the superconducting wire cannot be too high, the above annealing conditions can ensure that the core wire has sufficient softness after annealing.

[0067] Correspondingly, the present invention also provides a superconducting enameled wire, which is prepared by adopting the above-mentioned production process of superconducting wire and has good product quality.

[0068] Example 1

[0069] A production process for a superconducting wire comprises the following steps:

[0070] (1) Paying off the line;

[0071] (2) Forming: Rolling the incoming round wire into a core wire of set specifications;

[0072] (3) Cleaning: Clean the formed core wire;

[0073] (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace; the annealing temperature is 300°C and the annealing time is 90 seconds;

[0074] (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room and is painted with acetal insulating paint. Then it enters the baking furnace for baking. The baking time is 60s and the baking temperature is 280℃. The painting and baking are repeated 6 times. The thickness of the paint film formed each time is 20μm. Before each painting, the core wire is kept at a constant temperature: the temperature of the paint liquid in the paint tank and the temperature in the constant temperature painting room are both 40℃. The temperature of the core wire is 3℃ higher than the temperature of the constant temperature painting room.

[0075] (6) Inspection: inspect the core wire after painting and baking;

[0076] (7) Winding: Wind the core wire onto the finished spool.

[0077] Example 2

[0078] A production process for a superconducting wire comprises the following steps:

[0079] (1) Paying off the line;

[0080] (2) Forming: Rolling the incoming round wire into a core wire of set specifications;

[0081] (3) Cleaning: Clean the formed core wire;

[0082] (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace; the annealing temperature is 320°C and the annealing time is 80 seconds;

[0083] (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room and is painted with acetal insulating paint. It then enters the baking furnace for baking. The baking time is 80 seconds and the baking temperature is 260°C. The painting and baking are repeated 8 times. The thickness of the paint film formed each time is 10 μm. The core wire is kept at a constant temperature before each painting: the temperature of the paint liquid in the paint tank and the temperature in the constant temperature painting room are both 45°C. The temperature at which the core wire is kept at a constant temperature is 2°C higher than the temperature of the constant temperature painting room.

[0084] (6) Inspection: inspect the core wire after painting and baking;

[0085] (7) Winding: Wind the core wire onto the finished spool.

[0086] Example 3

[0087] A production process for a superconducting wire comprises the following steps:

[0088] (1) Paying off the line;

[0089] (2) Forming: Rolling the incoming round wire into a core wire of set specifications;

[0090] (3) Cleaning: Clean the formed core wire;

[0091] (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace; the annealing temperature is 280°C and the annealing time is 100s;

[0092] (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room for painting with acetal insulating paint and then enters the baking furnace for baking. The baking time is 40 s and the baking temperature is 300°C. The painting and baking are repeated 10 times. The thickness of the paint film formed each time is 80 μm. The core wire is kept at a constant temperature before each painting: the temperature of the paint liquid in the paint tank and the temperature in the constant temperature painting room are both 40°C. The temperature at which the core wire is kept at a constant temperature is 5°C higher than the temperature of the constant temperature painting room.

[0093] (6) Inspection: inspect the core wire after painting and baking;

[0094] (7) Winding: Wind the core wire onto the finished spool.

[0095] Example 4

[0096] This embodiment is basically the same as Embodiment 1, except that:

[0097] In step (1), each pay-off shaft is wound with a superconducting wire, and two adjacent superconducting wires are welded with ferromagnetic material to form a connection point;

[0098] Each of steps (2) to (7) has a wiring position identification step to identify the wiring position as a process node and record the real-time process data of each superconducting wire;

[0099] In step (7), the core wire is cut according to the connection position so that each superconducting wire is wound on a finished bobbin.

[0100] Specifically, a joint identification mechanism is used to identify the joint position; the joint identification mechanism includes a pressure sensor and a strong magnet connected to each other, and the strong magnet is used to generate suction to the joint to change the sensing data of the pressure sensor.

[0101] A production process of a superconducting wire according to an embodiment of the present invention and other structures and operations of the superconducting enameled wire are well known to those skilled in the art and will not be described in detail here.

[0102] In the description of this specification, the description with reference to the terms "embodiment", "example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0103] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A process for producing a superconducting wire, characterized in that: The following steps are involved: (1) Laying out the wire; (2) Forming: Rolling the incoming round wire into a shaped core wire of set specifications; (3) Cleaning: Clean the formed core wire; (4) Annealing: The core wire running at a uniform speed is annealed in an annealing furnace; (5) Painting and baking: The core wire running at a uniform speed enters the constant temperature painting room for painting and then enters the baking furnace for baking. The painting and baking are repeated 6 to 10 times. The core wire is kept at a constant temperature before each painting so that the temperature of the core wire matches the temperature of the paint liquid. (6) Inspection: inspect the core wire after painting and baking; (7) Winding: Winding the core wire onto the finished spool; In the step (5), the temperature at which the core wire is kept constant is higher than the temperature of the constant temperature painting room, the constant temperature painting room has a paint trough for receiving excess paint liquid, the core wire passes through the paint trough and moves upward through the thickness setting mold, a paint spraying tube is provided between the paint trough and the thickness setting mold, and the temperature of the paint liquid sprayed from the paint spraying tube is the same as the temperature in the constant temperature painting room; In the step (1), each pay-off shaft is wound with a superconducting wire, and two adjacent superconducting wires are welded to form a connection position; two adjacent superconducting wires are welded with ferromagnetic materials to form a connection position, and a joint identification mechanism is used to identify the connection position; the joint identification mechanism includes a pressure sensor and a strong magnet connected to each other, and the strong magnet is used to generate suction on the joint to change the sensing data of the pressure sensor; Each of the steps (2) to (7) has a wiring position identification step to identify the wiring position as a process node and record the real-time process data of each superconducting wire; In the step (7), the core wire is cut according to the connection position so that each superconducting wire is wound on a finished product bobbin.

2. The process for producing a superconducting wire according to claim 1, characterized in that: The temperature of the paint liquid in the paint tank and the temperature in the constant temperature painting room are both 40°C to 45°C; The temperature at which the core wire is kept constant is 2°C to 5°C higher than the temperature of the constant temperature painting room.

3. The process for producing a superconducting wire according to claim 1 or 2, characterized in that: In the step (5), the thickness of the paint film formed by each painting is the same, and the thickness of the paint film formed by each painting is 10 μm to 80 μm.

4. The process for producing a superconducting wire according to claim 1, characterized in that: The core wire is kept at a constant temperature in a constant temperature chamber, and the constant temperature chamber is connected to the constant temperature painting chamber so that the core wire enters the constant temperature painting chamber from the constant temperature chamber; The length of the temperature-regulating chamber is greater than 20 cm. The temperature-regulating chamber is divided into a cooling chamber and a constant temperature chamber. The core wire first enters the cooling chamber and then enters the constant temperature chamber.

5. The process for producing a superconducting wire according to claim 1, characterized in that: In the step (5), acetal insulating varnish is used, the baking time is 40s to 80s, and the baking temperature is 260°C to 300°C.

6. The process for producing a superconducting wire according to claim 1, characterized in that: In the step (4), the annealing temperature is 280° C. to 320° C., and the annealing time is 80 s to 100 s.

7. A superconducting enameled wire, characterized in that: The superconducting wire is prepared by the production process of the superconducting wire according to any one of claims 1 to 6.

Citation Information

Cited By

  • Production process of superconducting wire and superconducting enameled wire

    CN122025278A